Shape memory photo-thermal ice preventing and removing super-hydrophobic material and preparation method thereof
By combining epoxy resin, inorganic photothermal nanoparticles and metal nanoparticles, shape memory photothermal anti-icing superhydrophobic materials are prepared, which solves the high cost and low efficiency of the existing ice-proof methods, and realizes the low temperature environment Highly efficient deicing and good durability, suitable for anti-icing applications in a variety of equipment.
Patent Information
- Application Number
- CN202411180935.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
Existing anti-icing methods such as electric heat deicing, mechanical deicing and chemical reagent deicing have problems such as high cost, low efficiency, environmental pollution and equipment damage, and the photothermal superhydrophobic material process is complex and not practical.
A shape memory photothermal anti-icing superhydrophobic material is prepared by combining epoxy resin, inorganic photothermal nanoparticles and metal nanoparticles to form a composite photothermal surface with micro-nano structure, and modified epoxy The resin solution is hydrophobized to achieve high-efficiency photothermal conversion in the wavelength range of 400 to 2000 nm.
It realizes the delayed ice formation and rapid deicing of materials in low temperature environments, and has good shape memory function, mechanical and chemical durability and anti-ultraviolet aging performance. It is suitable for anti-icing applications of a variety of equipment.
Smart Images

Figure CN119060392A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of anti-icing material preparation, and in particular to a shape memory photothermal anti-icing super-hydrophobic material and a preparation method thereof. Background Art
[0002] Icing is a common phenomenon in nature. The surfaces of various aerospace equipment (helicopters, drones, manned spacecraft, etc.) working in low-temperature environments, high-voltage transmission lines, wind turbines, high-speed railways operating in cold regions, and other equipment are prone to ice. When the surface of the equipment is frozen, it is easy to cause mechanical and electrical failures, affecting the normal operation of the equipment, posing huge safety hazards, and even leading to major accidents. To this end, researchers have proposed many solutions, such as mechanical deicing, electric heating deicing, and spraying chemical reagents for deicing. However, these methods have the disadvantages of high cost, low efficiency, environmental pollution, and easy damage to the surface of the equipment, and are not widely applicable. Therefore, it is very necessary to develop an economical, efficient, applicable, and equipment-friendly anti-icing method.
[0003] Different from the previous active deicing methods such as electric deicing, mechanical deicing, and chemical reagent deicing, ice is not easy to form and accumulate on the surface of superhydrophobic materials, and can be passively anti-icing. Photothermal materials can effectively prevent ice formation when the surface temperature of the material is higher than the freezing temperature, and even effectively melt the ice accumulated on the surface of the material. Photothermal superhydrophobic materials are prepared by combining superhydrophobic materials with photothermal materials. Combining passive anti-icing with active deicing is considered to be an economical, efficient, and environmentally friendly anti-icing / deicing method. Yin et al. (Yin X, Zhang Y, Wang D, et al. Integration of self-lubrication and near-infrared photothermogenesis for excellent anti-icing / deicing performance [J]. Advanced Functional Materials, 2015, 25 (27): 4237-4245.) poured a mixture of magnetic Fe3O4 nanoparticles and PDMS onto a self-assembled polystyrene microsphere template. After curing and removing the template, a photothermal surface with a porous structure was successfully prepared. Subsequently, a self-lubricating coating with photothermal conversion properties was constructed by injecting a perfluoropolyether lubricant into the porous structure. When the surface was covered with ice / frost, the ice / frost could be removed under near-infrared laser irradiation (808 nm, 1000 mW / cm 2 ) to melt quickly. This method is relatively complicated and requires light of a specific wavelength to achieve de-icing, which is not practical. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a shape memory photothermal anti-icing super-hydrophobic material and a preparation method thereof. The preparation method provided by the present invention has a simple process, and the obtained shape memory photothermal anti-icing super-hydrophobic material has a light absorption rate greater than 90% in the wavelength range of 400 to 2000nm, which is more practical.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a shape memory photothermal anti-icing super-hydrophobic material, comprising the following steps:
[0007] Mixing epoxy resin, curing agent, reactive diluent and organic solvent to obtain epoxy resin substrate solution;
[0008] Semi-curing the epoxy resin substrate solution to obtain a semi-cured epoxy resin substrate;
[0009] Using hot embossing, a microstructure is formed on the surface of the semi-cured epoxy resin substrate to obtain an epoxy resin substrate with a microstructure;
[0010] mixing epoxy resin, curing agent, organic solvent and inorganic photothermal nanoparticles to obtain a spray solution;
[0011] The spraying solution is sprayed onto the microstructure of the epoxy resin substrate having the microstructure, and after curing, the epoxy resin substrate having the micro-nanostructure is obtained;
[0012] sputtering metal on the micro-nano structure of the epoxy resin substrate having the micro-nano structure to obtain a substrate having a metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface;
[0013] mixing an epoxy resin, a curing agent, an organic solvent and a hydrophobic modifier to obtain a modified epoxy resin solution;
[0014] The substrate having the metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface is immersed in the modified epoxy resin solution and heated to obtain the shape memory photothermal anti-icing superhydrophobic material.
[0015] Preferably, in the epoxy resin substrate solution, the epoxy resin is a bisphenol A epoxy resin, and the epoxy equivalent of the bisphenol A epoxy resin is 175 to 185 g / mol;
[0016] The curing agent is an amine curing agent, an acid anhydride curing agent or a polyol curing agent; the amine curing agent is polyetheramine D230, diethylenetriamine or triethylenetetramine; the acid anhydride curing agent is phthalic anhydride or adipic anhydride; the polyol curing agent is polyether polyol;
[0017] The active diluent is polypropylene glycol diglycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, ethylene glycol bisglycidyl ether or resorcinol bisglycidyl ether;
[0018] The organic solvent is N,N-dimethylformamide, glycol ether or phenylethanol;
[0019] The mass ratio of epoxy resin, curing agent, active diluent and organic solvent is 5:1-3:0.5-1:1-4.
[0020] Preferably, the semi-curing temperature is 50-70° C. and the time is 1.5-2.5 hours.
[0021] Preferably, the forming of the microstructure on the semi-cured epoxy resin substrate by hot stamping comprises the following steps: placing a template with a microstructure on the top layer of the semi-cured resin, pressing to fully combine the template and the semi-cured resin, and curing at 70-90° C. for 0.5-1.5 h and at 90-110° C. for 0.5-1.5 h in sequence; after curing, separating the template from the epoxy resin at 50-70° C.;
[0022] The mesh number of the template with microstructure is 200 to 1000 mesh;
[0023] The material of the template with microstructure is fiber cloth, copper mesh or stainless steel mesh.
[0024] Preferably, in the spray solution, the epoxy resin is a bisphenol A epoxy resin, and the epoxy equivalent of the bisphenol A epoxy resin is 175 to 185 g / mol;
[0025] The curing agent is an amine curing agent, an acid anhydride curing agent or a polyol curing agent; the amine curing agent is polyetheramine D230, diethylenetriamine or triethylenetetramine; the acid anhydride curing agent is phthalic anhydride or adipic anhydride; the polyol curing agent is polyether polyol;
[0026] The organic solvent is N,N-dimethylformamide, glycol ether or phenylethanol;
[0027] The inorganic photothermal nanoparticles are titanium carbide nanoparticles, silicon carbide nanoparticles or carbon nanotubes;
[0028] The mass ratio of epoxy resin, curing agent, organic solvent and inorganic photothermal nanoparticles is 3:0.6-1.8:15-45:0.3-1.2.
[0029] Preferably, the curing temperature is 90-110° C. and the curing time is 0.5-1.5 h.
[0030] Preferably, the sputtering thickness of the metal is 3-5 nm, the metal is copper or iron, and the sputtering parameters include: target purity is 99.9%, current intensity is 30-50 mA, and sputtering time is 30-120 s.
[0031] Preferably, in the modified epoxy resin solution, the epoxy resin is a bisphenol A epoxy resin, and the epoxy equivalent of the bisphenol A epoxy resin is 175 to 185 g / mol;
[0032] The curing agent is an amine curing agent, an acid anhydride curing agent or a polyol curing agent; the amine curing agent is polyetheramine D230, diethylenetriamine or triethylenetetramine; the acid anhydride curing agent is phthalic anhydride or adipic anhydride; the polyol curing agent is polyether polyol;
[0033] The organic solvent is N,N-dimethylformamide, glycol ether or phenylethanol;
[0034] The hydrophobic modifier is heptadecafluorosilane, fatty acid or alkyl silane coupling agent;
[0035] The mass ratio of epoxy resin, curing agent, organic solvent and hydrophobic modifier is 5:1-3:15-45:0.05-0.15.
[0036] Preferably, the heating temperature is 90-110° C. and the heating time is 0.5-1.5 h.
[0037] The present invention also provides a shape memory photothermal anti-icing super-hydrophobic material obtained by the preparation method described in the above technical solution.
[0038] The invention provides a method for preparing a shape memory photothermal anti-icing super-hydrophobic material, comprising the following steps: mixing an epoxy resin, a curing agent, an active diluent and an organic solvent to obtain an epoxy resin substrate solution; semi-curing the epoxy resin substrate solution to obtain a semi-cured epoxy resin substrate; using hot stamping to form a microstructure on the surface of the semi-cured epoxy resin substrate to obtain an epoxy resin substrate with a microstructure; mixing the epoxy resin, the curing agent, the organic solvent and inorganic photothermal nanoparticles to obtain a spray solution; spraying the spray solution onto the epoxy resin substrate with a microstructure The microstructure of the resin substrate is cured to obtain an epoxy resin substrate with a micro-nano structure; metal is sputtered on the micro-nano structure of the epoxy resin substrate with the micro-nano structure to obtain a substrate with a metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface; epoxy resin, a curing agent, an organic solvent and a hydrophobic modifier are mixed to obtain a modified epoxy resin solution; the substrate with the metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface is immersed in the modified epoxy resin solution and heated to obtain the shape memory photothermal anti-icing super hydrophobic material.
[0039] Compared with the prior art, the present invention has the following advantages:
[0040] (1) The shape memory photothermal anti-icing superhydrophobic material prepared by the present invention has a shape memory function. By heating, the material is heated to above the deformable temperature, and then an external load is applied to change its shape. After maintaining the load and cooling, the material can obtain a temporary shape, and finally release the stress by heating again to restore it to its original shape. The material has a photothermal effect and therefore also has a light stimulus response characteristic. It can respond to light and heat stimulation to perform shape memory and recovery, and the shape recovery rate is close to 100%.
[0041] (2) The shape memory photothermal anti-icing super-hydrophobic material prepared by the present invention utilizes the synergistic photothermal properties of inorganic photothermal nanoparticles and metal nanoparticles to make the surface of the shape memory photothermal anti-icing super-hydrophobic material have good photothermal conversion performance, and the light absorption rate is greater than 90% in the wavelength range of 400 to 2000 nm.
[0042] (3) The shape memory photothermal anti-icing superhydrophobic material prepared by the present invention has good anti-icing performance, can effectively delay the freezing time in a low temperature environment of -20°C, and can further extend the freezing time under light conditions. The deicing test results show that under the illumination intensity of 1 sun, the surface temperature of the material increases rapidly and the deicing efficiency is significantly improved. Even under lower ambient temperatures and weaker light intensity, the material still has good deicing performance.
[0043] (4) The shape memory photothermal anti-icing superhydrophobic material prepared by the present invention has good mechanical and chemical durability, anti-ultraviolet aging performance and good self-cleaning performance, providing the possibility for long-term outdoor use. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The micro-nano morphology and super-hydrophobic state of the shape memory photothermal anti-icing super-hydrophobic material obtained in Example 1;
[0045] Figure 2 The surface contact angle of the shape memory photothermal anti-icing superhydrophobic material with different contents of titanium carbide nanoparticles in Example 1;
[0046] Figure 3 This is a diagram of the shape memory recovery process of the shape memory photothermal anti-icing superhydrophobic material obtained in Example 2;
[0047] Figure 4 It is a diagram showing the melting process of ice on the surface of the shape memory photothermal anti-icing superhydrophobic material obtained in Example 3 under different light intensities and different ambient temperatures;
[0048] Figure 5The change in surface contact angle of the shape memory photothermal anti-icing superhydrophobic material obtained in Example 1 under ultraviolet light irradiation at different times (a) and the self-cleaning process diagram (b). DETAILED DESCRIPTION
[0049] The present invention provides a method for preparing a shape memory photothermal anti-icing super-hydrophobic material, comprising the following steps:
[0050] Mixing epoxy resin, curing agent, reactive diluent and organic solvent to obtain epoxy resin substrate solution;
[0051] Semi-curing the epoxy resin substrate solution to obtain a semi-cured epoxy resin substrate;
[0052] Using hot embossing, a microstructure is formed on the surface of the semi-cured epoxy resin substrate to obtain an epoxy resin substrate with a microstructure;
[0053] mixing epoxy resin, curing agent, organic solvent and inorganic photothermal nanoparticles to obtain a spray solution;
[0054] The spraying solution is sprayed onto the microstructure of the epoxy resin substrate having the microstructure, and after curing, the epoxy resin substrate having the micro-nanostructure is obtained;
[0055] sputtering metal on the micro-nano structure of the epoxy resin substrate having the micro-nano structure to obtain a substrate having a metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface;
[0056] mixing an epoxy resin, a curing agent, an organic solvent and a hydrophobic modifier to obtain a modified epoxy resin solution;
[0057] The substrate having the metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface is immersed in the modified epoxy resin solution and heated to obtain the shape memory photothermal anti-icing superhydrophobic material.
[0058] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0059] The invention mixes epoxy resin, curing agent, active diluent and organic solvent to obtain epoxy resin substrate solution.
[0060] In the present invention, the epoxy resin is preferably bisphenol A epoxy resin, and the epoxy equivalent of the bisphenol A epoxy resin is preferably 175 to 185 g / mol. In a specific embodiment of the present invention, the bisphenol A epoxy resin is preferably bisphenol A epoxy resin E54.
[0061] In the present invention, the curing agent is preferably an amine curing agent, an anhydride curing agent or a polyol curing agent, and is more preferably an amine curing agent. In the present invention, the amine curing agent is preferably polyetheramine D230, (DETA), diethylenetriamine (DETA) or triethylenetetramine (TETA), and is more preferably polyetheramine D230. In the present invention, the anhydride curing agent is preferably phthalic anhydride or adipic anhydride. In the present invention, the polyol curing agent is preferably polyether polyol.
[0062] In the present invention, the reactive diluent is preferably polypropylene glycol diglycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, ethylene glycol bisglycidyl ether or resorcinol bisglycidyl ether, and more preferably polypropylene glycol diglycidyl ether.
[0063] In the present invention, the organic solvent is preferably N,N-dimethylformamide, glycol ether or phenylethanol, and more preferably N,N-dimethylformamide; the glycol ether is preferably butyl triglycol ether.
[0064] In the present invention, the mass ratio of the epoxy resin, the curing agent, the reactive diluent and the organic solvent in the epoxy resin substrate solution is preferably 5:1-3:0.5-1:1-4, and more preferably 5:2:1:3.
[0065] In the present invention, the epoxy resin, curing agent, reactive diluent and organic solvent are preferably mixed under magnetic stirring, and the magnetic stirring time is preferably 0.5 to 1.5 hours, and more preferably 1 hour. After the mixing, the present invention preferably further comprises vacuum pumping and degassing, and the vacuum pumping and degassing time is preferably 10 to 20 minutes, and more preferably 15 minutes.
[0066] In the present invention, the semi-curing temperature is preferably 50 to 70° C., more preferably 60° C., and the time is preferably 1.5 to 2.5 hours, more preferably 2 hours.
[0067] After obtaining the semi-cured epoxy resin substrate, the present invention uses hot embossing to form a microstructure on the surface of the semi-cured epoxy resin substrate to obtain an epoxy resin substrate with a microstructure.
[0068] In the present invention, the formation of microstructures on the semi-cured epoxy resin substrate by hot stamping preferably includes the following steps: placing a template with a microstructure on the top layer of the semi-cured resin, pressing to fully combine the template and the semi-cured resin, curing at 70-90°C for 0.5-1.5h, and curing at 90-110°C for 0.5-1.5h; after curing, separating the template from the epoxy resin at 50-70°C; more preferably, placing a template with a microstructure on the top layer of the semi-cured resin, pressing to fully combine the template and the semi-cured resin, curing at 80°C for 1h, and curing at 100°C for 1h; after curing, separating the template from the epoxy resin at 60°C. In the present invention, the mesh number of the template with a microstructure is preferably 200-1000 meshes. In the present invention, the material of the template with a microstructure is preferably fiber cloth, copper mesh or stainless steel mesh, and more preferably fiber cloth.
[0069] The present invention utilizes hot embossing to construct a micron structure on the surface of a material.
[0070] The invention mixes epoxy resin, curing agent, organic solvent and inorganic photothermal nanoparticles to obtain a spraying solution.
[0071] In the present invention, the epoxy resin, curing agent and organic solvent in the spray solution are consistent with those in the epoxy resin substrate solution, and are not repeated here. In the present invention, the inorganic photothermal nanoparticles are preferably titanium carbide nanoparticles, silicon carbide nanoparticles or carbon nanotubes, and are further preferably titanium carbide nanoparticles. In the present invention, in the spray solution, the mass ratio of epoxy resin, curing agent, organic solvent and inorganic photothermal nanoparticles is preferably 3:0.6~1.8:15~45:0.3~1.2, and is further preferably 3:1:30:0.3.
[0072] In the present invention, the epoxy resin, curing agent, organic solvent and inorganic photothermal nanoparticles are preferably mixed under the condition of magnetic stirring, and the magnetic stirring time is preferably 0.5 to 1.5 hours, and more preferably 1 hour.
[0073] After obtaining the spraying solution, the present invention sprays the spraying solution onto the microstructure of the epoxy resin substrate with microstructure, and obtains the epoxy resin substrate with micro-nano structure after curing.
[0074] In the present invention, the spraying equipment is preferably a spray gun. In the present invention, the spraying amount of the spraying solution is preferably 10 to 12 m2 per liter of spraying solution. 2 .
[0075] In the present invention, the curing temperature is preferably 90 to 110° C., more preferably 100° C., and the curing time is preferably 0.5 to 1.5 h, more preferably 1 h.
[0076] The present invention adds inorganic photothermal nanoparticles into the spraying solution, introduces a nanostructure on the constructed microstructure, and then constructs a micro-nano structure. The micro-nano hierarchical structure is conducive to forming a more stable super-hydrophobic surface with a larger contact angle; at the same time, it can also increase the wear resistance of the material, because the primary structure is destroyed during the application process, and there is also a secondary structure.
[0077] After obtaining the epoxy resin substrate with micro-nano structure, the present invention sputters metal on the micro-nano structure of the epoxy resin substrate with micro-nano structure to obtain a substrate with a metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface.
[0078] In the present invention, the sputtering thickness of the metal is preferably 3 to 5 nm. In the present invention, the metal is preferably copper or iron, and more preferably copper. In the present invention, the sputtering is preferably magnetron sputtering, and the magnetron sputtering is preferably performed in a plasma magnetron sputtering apparatus. In the present invention, the parameters of the sputtering include: the target purity is preferably 99.9%, the current intensity is preferably 30 to 50 mA, and the sputtering time is preferably 30 to 120 s.
[0079] In the present invention, metal deposition improves wear resistance and more importantly can enhance the photothermal effect to enhance the deicing effect.
[0080] The invention mixes epoxy resin, curing agent, organic solvent and hydrophobic modifier to obtain modified epoxy resin solution.
[0081] In the present invention, the epoxy resin, curing agent and organic solvent in the modified epoxy resin solution are consistent with those in the epoxy resin substrate solution, and are not repeated here. In the present invention, the hydrophobic modifier is preferably heptafluorosilane, fatty acid or alkylsilane coupling agent, and is further preferably heptafluorosilane. In the present invention, the heptafluorosilane is preferably heptafluorodecyltrimethoxysilane. In the present invention, the fatty acid preferably includes one or more of lauric acid, palmitic acid and stearic acid. In the present invention, the alkylsilane coupling agent preferably includes one or more of octadecyltrichlorosilane, octadecyltriethoxysilane and 3-(methacryloyloxy)propyltrimethoxysilane.
[0082] In the present invention, the mass ratio of the epoxy resin, the curing agent, the organic solvent and the hydrophobic modifier in the modified epoxy resin solution is preferably 5:1-3:15-45:0.05-0.15, and more preferably 5:2:20:0.05.
[0083] In the present invention, the epoxy resin, curing agent, organic solvent and hydrophobic modifier are preferably mixed under magnetic stirring, and the magnetic stirring time is preferably 1 to 2 hours, more preferably 1.5 hours.
[0084] The present invention adds a hydrophobic modifier into the modified epoxy resin solution, which can make the surface of the material more hydrophobic, and the hydrophobicity also makes the material more difficult to be covered with ice.
[0085] After obtaining the modified epoxy resin solution, the present invention immerses the substrate having the metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface into the modified epoxy resin solution and heats it to obtain the shape memory photothermal anti-icing superhydrophobic material.
[0086] In the present invention, the immersion time is preferably 4 to 6 minutes, more preferably 5 minutes.
[0087] In the present invention, the heating temperature is preferably 90 to 110° C., more preferably 100° C., and the heating time is preferably 0.5 to 1.5 h, more preferably 1 h.
[0088] The present invention also provides a shape memory photothermal anti-icing super-hydrophobic material obtained by the preparation method described in the above technical solution.
[0089] In the present invention, the shape memory photothermal anti-icing superhydrophobic material can be applied to power grids, wind turbines, high-speed railways, aviation or ships.
[0090] The shape memory photothermal anti-icing super-hydrophobic material and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0091] Example 1
[0092] (1) Preparation of semi-cured epoxy resin substrate
[0093] Epoxy resin (bisphenol A epoxy resin E54), curing agent (polyetheramine D230), active diluent (polypropylene glycol diglycidyl ether) and organic solvent (N,N-dimethylformamide) were mixed in a mass ratio of 5:2:1:3, and stirred with a glass rod until the resin was completely dissolved to obtain an epoxy resin prepolymer. The prepolymer was magnetically stirred for 1 hour to make the solution evenly mixed. Then, vacuum evacuated for 15 minutes to remove bubbles in the mixed solution. The mixed solution was placed in an oven and cured at 60°C for 2 hours to obtain a semi-cured epoxy resin substrate.
[0094] (2) Construction of surface microstructure
[0095] A fiber cloth with a microstructure (mesh size of 200) was placed as a template on the top layer of the semi-cured epoxy resin substrate prepared in step (1), and pressed to fully combine the fiber cloth and the semi-cured epoxy resin substrate, and cured at 80° C. for 1 hour and 100° C. for 1 hour. After the curing was completed, the template was separated from the epoxy resin at 60° C. to obtain an epoxy resin substrate with a microstructure.
[0096] (3) Construction of surface micro-nanostructures
[0097] An epoxy resin (bisphenol A type epoxy resin E54), a curing agent (polyetheramine D230), an organic solvent (N,N-dimethylformamide) and titanium carbide nanoparticles are mixed in a mass ratio of 3:1:30:0.3, and magnetically stirred for 1 hour to obtain a spray solution; the spray solution is sprayed onto the microstructure of the epoxy resin substrate with a microstructure obtained in step (2) with a spray gun, and heated in an oven at 100° C. for 1 hour to obtain an epoxy resin substrate with a micro-nano structure.
[0098] (4) Surface deposition of metal particles
[0099] Then, the epoxy resin substrate with micro-nano structure obtained in step (3) is placed in a plasma magnetron sputtering instrument, the sputtering current intensity is adjusted to 30 mA, and the sputtering time is adjusted to 30 s, and copper is sputtered onto the micro-nano structure of the epoxy resin substrate with micro-nano structure to obtain a substrate with a copper / titanium carbide / epoxy resin composite photothermal surface.
[0100] (5) Surface hydrophobic modification
[0101] Epoxy resin (bisphenol A epoxy resin E54), curing agent (polyetheramine D230), organic solvent (N,N-dimethylformamide) and heptadecafluorodecyltrimethoxysilane were mixed in a mass ratio of 5:2:20:0.05 and magnetically stirred for 1.5 hours to obtain a modified epoxy resin solution.
[0102] The substrate with the copper / titanium carbide / epoxy resin composite photothermal surface prepared in step (4) was immersed in a modified epoxy resin solution for 5 minutes, and then placed in an oven and heated at 100° C. for 1 hour to obtain a shape memory photothermal anti-icing superhydrophobic material.
[0103] Anti-icing test of the obtained shape memory photothermal anti-icing superhydrophobic material
[0104] The shape memory photothermal anti-icing and deicing superhydrophobic material prepared in step (5) is subjected to anti-icing and deicing tests under different temperatures and different lighting conditions.
[0105] Example 2
[0106] (1) Preparation of semi-cured epoxy resin substrate
[0107] Epoxy resin (bisphenol A epoxy resin E54), curing agent (polyetheramine D230), active diluent (polypropylene glycol diglycidyl ether) and organic solvent (N,N-dimethylformamide) were mixed in a mass ratio of 5:2:1:3, and stirred with a glass rod until the resin was completely dissolved to obtain an epoxy resin prepolymer. The prepolymer was magnetically stirred for 1 hour to make the solution evenly mixed. Then, vacuum evacuated for 15 minutes to remove bubbles in the mixed solution. The mixed solution was placed in an oven and cured at 60°C for 2 hours to obtain a semi-cured epoxy resin substrate.
[0108] (2) Construction of surface microstructure
[0109] A fiber cloth with a microstructure (mesh size of 200) was placed as a template on the top layer of the semi-cured epoxy resin substrate prepared in step (1), and pressed to fully combine the fiber cloth and the semi-cured epoxy resin substrate, and cured at 80° C. for 1 hour and 100° C. for 1 hour. After the curing was completed, the template was separated from the epoxy resin at 60° C. to obtain an epoxy resin substrate with a microstructure.
[0110] (3) Construction of surface micro-nanostructures
[0111] Epoxy resin (bisphenol A type epoxy resin E54), curing agent (polyetheramine D230), organic solvent (N,N-dimethylformamide) and titanium carbide nanoparticles are mixed in a mass ratio of 3:1:30:0.6, and magnetically stirred for 1 hour to obtain a spray solution; the spray solution is sprayed onto the microstructure of the epoxy resin substrate with microstructure obtained in step (2) with a spray gun, and heated in an oven at 100° C. for 1 hour to obtain the epoxy resin substrate with micro-nano structure.
[0112] (4) Surface deposition of metal particles
[0113] Then, the epoxy resin substrate with micro-nano structure obtained in step (3) is placed in a plasma magnetron sputtering instrument, the sputtering current intensity is adjusted to 40 mA, the sputtering time is adjusted to 60 s, and copper is sputtered onto the substrate surface to obtain a substrate with a copper / titanium carbide / epoxy resin composite photothermal surface.
[0114] (5) Surface hydrophobic modification
[0115] Epoxy resin (bisphenol A epoxy resin E54), curing agent (polyetheramine D230), organic solvent (N,N-dimethylformamide) and heptadecafluorodecyltrimethoxysilane were mixed in a mass ratio of 5:2:20:0.1 and magnetically stirred for 1.5 hours to obtain a modified epoxy resin solution.
[0116] The substrate with the copper / titanium carbide / epoxy resin composite photothermal surface prepared in step (4) was immersed in a modified epoxy resin solution for 5 minutes, and then placed in an oven and heated at 100° C. for 1 hour to obtain a shape memory photothermal anti-icing superhydrophobic material.
[0117] Anti-icing test of the obtained shape memory photothermal anti-icing superhydrophobic material
[0118] The shape memory photothermal anti-icing and deicing superhydrophobic material prepared in step (5) is subjected to anti-icing and deicing tests under different temperatures and different lighting conditions.
[0119] Example 3
[0120] (1) Preparation of semi-cured epoxy resin substrate
[0121] Epoxy resin (bisphenol A epoxy resin E54), curing agent (polyetheramine D230), active diluent (polypropylene glycol diglycidyl ether) and organic solvent (N,N-dimethylformamide) were mixed in a mass ratio of 5:2:1:3, and stirred with a glass rod until the resin was completely dissolved to obtain an epoxy resin prepolymer. The prepolymer was magnetically stirred for h to make the solution evenly mixed. Then, vacuum evacuated for 15 minutes to remove bubbles in the mixed solution. The mixed solution was placed in an oven and cured at 60°C for 2 hours to obtain a semi-cured epoxy resin substrate.
[0122] (2) Construction of surface microstructure
[0123] A fiber cloth with a microstructure (mesh size of 200) was placed as a template on the top layer of the semi-cured epoxy resin substrate prepared in step (1), and pressed to fully combine the fiber cloth and the semi-cured epoxy resin substrate, and cured at 80° C. for 1 hour and 100° C. for 1 hour. After the curing was completed, the template was separated from the epoxy resin at 60° C. to obtain an epoxy resin substrate with a microstructure.
[0124] (3) Construction of surface micro-nanostructures
[0125] An epoxy resin (bisphenol A type epoxy resin E54), a curing agent (polyetheramine D230), an organic solvent (N,N-dimethylformamide) and titanium carbide nanoparticles are mixed in a mass ratio of 3:1:30:0.9, and magnetically stirred for 1 hour to obtain a spray solution; the spray solution is sprayed onto the microstructure of the epoxy resin substrate with a microstructure obtained in step (2) with a spray gun, and heated in an oven at 100° C. for 1 hour to obtain an epoxy resin substrate with a micro-nano structure.
[0126] (4) Surface deposition of metal particles
[0127] Then, the epoxy resin substrate with micro-nano structure obtained in step (3) is placed in a plasma magnetron sputtering instrument, the sputtering current intensity is adjusted to 50 mA, the sputtering time is adjusted to 90 s, and copper is sputtered onto the substrate surface to obtain a substrate with a copper / titanium carbide / epoxy resin composite photothermal surface.
[0128] (5) Surface hydrophobic modification
[0129] Epoxy resin (bisphenol A epoxy resin E54), curing agent (polyetheramine D230), organic solvent (N,N-dimethylformamide) and heptadecafluorodecyltrimethoxysilane were mixed in a mass ratio of 5:2:20:0.15 and magnetically stirred for 1.5 hours to obtain a modified epoxy resin solution.
[0130] The substrate with the copper / titanium carbide / epoxy resin composite photothermal surface prepared in step (4) was immersed in a modified epoxy resin solution for 5 minutes, and then placed in an oven and heated at 100° C. for 1 hour to obtain a shape memory photothermal anti-icing superhydrophobic material.
[0131] Anti-icing test of the obtained shape memory photothermal superhydrophobic material
[0132] The shape memory photothermal anti-icing and deicing superhydrophobic material prepared in step (5) is subjected to anti-icing and deicing tests under different temperatures and different lighting conditions.
[0133] In summary, the present invention first prepares a shape memory semi-cured epoxy resin substrate, transfers a template with a microstructure to the semi-cured epoxy resin substrate by a hot embossing method, then uses a spraying method to obtain a micro-nano hierarchical structure on the microstructure, and then uses sputtering to plate a layer of metal particles on the surface of the micro-nano hierarchical structure to obtain a synergistic photothermal effect, and finally uses a modified epoxy resin solution for immersion modification to prepare a shape memory epoxy resin photothermal superhydrophobic material, and the surface forms a micro-nano morphology superhydrophobic state. Figure 1 The micro-nano morphology and super-hydrophobic state of the shape memory photothermal anti-icing super-hydrophobic material obtained in Example 1.
[0134] By changing the content of titanium carbide nanoparticles relative to epoxy resin in the spray solution in Example 1, super-hydrophobic surfaces with different morphologies and different wettabilities can be obtained. Figure 2 As shown, Figure 2 is the surface contact angle of the shape memory photothermal anti-icing superhydrophobic material with different contents of titanium carbide nanoparticles in Example 1, Figure 2 It can be seen that the maximum contact angle of the surface is as high as 162°.
[0135] The prepared shape memory photothermal anti-icing super-hydrophobic material can respond to light stimulation to perform shape memory and recovery. The shape memory photothermal anti-icing super-hydrophobic material obtained in Example 2 will bend and curl under light stimulation. Figure 3 This is a diagram of the shape memory recovery process of the shape memory photothermal anti-icing superhydrophobic material obtained in Example 2. Figure 3It can be seen that the shape memory photothermal anti-icing superhydrophobic material obtained in Example 2 will be bent and curled under light stimulation, and its temporary shape will be obtained after maintaining the external load and cooling, and the shape fixation rate is close to 100%; by reasonably setting the original shape and the temporary shape, it can be flexibly used on the surface of various equipment, and the surface still has superhydrophobicity after 100 times of shape memory.
[0136] An ice layer with a thickness of about 1.5 mm was frozen on the surface of the shape memory photothermal anti-icing superhydrophobic material obtained in Example 3. The sample surface was irradiated with different light intensities, and the melting process of the ice layer on the sample surface was recorded. The melting time was given. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that: as the ambient temperature continues to drop, the time it takes for the ice to melt gradually increases. However, due to the unchanged light intensity, the synergistic photothermal properties of titanium carbide photothermal nanoparticles and metal nanoparticles can still quickly convert light energy into thermal energy, allowing the ice to still melt quickly.
[0137] It has good mechanical and chemical durability, anti-UV aging and self-cleaning properties, making it possible for long-term outdoor use.
[0138] Figure 5 The surface contact angle change (a) and the self-cleaning process diagram (b) of the shape memory photothermal anti-icing superhydrophobic material obtained in Example 1 under ultraviolet light irradiation at different times are shown in FIG. Figure 5 It can be seen that after fourteen days of UV accelerated aging test, the contact angle on the surface of the shape memory photothermal anti-icing superhydrophobic material has hardly changed and is stable at around 160°.
[0139] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a shape memory photothermal anti-icing super-hydrophobic material, It is characterized in that The following steps are involved: Mixing epoxy resin, curing agent, reactive diluent and organic solvent to obtain epoxy resin substrate solution; Semi-curing the epoxy resin substrate solution to obtain a semi-cured epoxy resin substrate; Using hot embossing, a microstructure is formed on the surface of the semi-cured epoxy resin substrate to obtain an epoxy resin substrate with a microstructure; mixing epoxy resin, curing agent, organic solvent and inorganic photothermal nanoparticles to obtain a spray solution; The spraying solution is sprayed onto the microstructure of the epoxy resin substrate having the microstructure, and after curing, the epoxy resin substrate having the micro-nanostructure is obtained; sputtering metal on the micro-nano structure of the epoxy resin substrate having the micro-nano structure to obtain a substrate having a metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface; mixing an epoxy resin, a curing agent, an organic solvent and a hydrophobic modifier to obtain a modified epoxy resin solution; The substrate having the metal / inorganic photothermal nanoparticle / epoxy resin composite photothermal surface is immersed in the modified epoxy resin solution and heated to obtain the shape memory photothermal anti-icing superhydrophobic material.
2. The preparation method according to claim 1, It is characterized in that In the epoxy resin substrate solution, the epoxy resin is a bisphenol A epoxy resin, and the epoxy equivalent of the bisphenol A epoxy resin is 175 to 185 g / mol; The curing agent is an amine curing agent, an acid anhydride curing agent or a polyol curing agent; the amine curing agent is polyetheramine D230, diethylenetriamine or triethylenetetramine; the acid anhydride curing agent is phthalic anhydride or adipic anhydride; the polyol curing agent is polyether polyol; The active diluent is polypropylene glycol diglycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, ethylene glycol bisglycidyl ether or resorcinol bisglycidyl ether; The organic solvent is N,N-dimethylformamide, glycol ether or phenylethanol; The mass ratio of epoxy resin, curing agent, active diluent and organic solvent is 5:1-3:0.5-1:1-4.
3. The preparation method according to claim 1 or 2, It is characterized in that The semi-curing temperature is 50-70° C. and the time is 1.5-2.5 hours.
4. The preparation method according to claim 1, It is characterized in that The method of forming a microstructure on the semi-cured epoxy resin substrate by hot stamping comprises the following steps: placing a template with a microstructure on the top layer of the semi-cured resin, pressing to fully combine the template and the semi-cured resin, and curing at 70 to 90° C. for 0.5 to 1.5 hours and at 90 to 110° C. for 0.5 to 1.5 hours in sequence; after curing, separating the template from the epoxy resin at 50 to 70° C.; The mesh number of the template with microstructure is 200 to 1000 mesh; The material of the template with microstructure is fiber cloth, copper mesh or stainless steel mesh.
5. The preparation method according to claim 1, It is characterized in that In the spraying solution, the epoxy resin is a bisphenol A epoxy resin, and the epoxy equivalent of the bisphenol A epoxy resin is 175 to 185 g / mol; The curing agent is an amine curing agent, an acid anhydride curing agent or a polyol curing agent; the amine curing agent is polyetheramine D230, diethylenetriamine or triethylenetetramine; the acid anhydride curing agent is phthalic anhydride or adipic anhydride; the polyol curing agent is polyether polyol; The organic solvent is N,N-dimethylformamide, glycol ether or phenylethanol; The inorganic photothermal nanoparticles are titanium carbide nanoparticles, silicon carbide nanoparticles or carbon nanotubes; The mass ratio of epoxy resin, curing agent, organic solvent and inorganic photothermal nanoparticles is 3:0.6-1.8:15-45:0.3-1.
2.
6. The preparation method according to claim 1 or 5, It is characterized in that The curing temperature is 90-110° C. and the curing time is 0.5-1.5 h.
7. The preparation method according to claim 1, It is characterized in that The sputtering thickness of the metal is 3-5 nm, the metal is copper or iron, and the sputtering parameters include: target material purity is 99.9%, current intensity is 30-50 mA, and sputtering time is 30-120 s.
8. The preparation method according to claim 1, It is characterized in that In the modified epoxy resin solution, the epoxy resin is a bisphenol A epoxy resin, and the epoxy equivalent of the bisphenol A epoxy resin is 175 to 185 g / mol; The curing agent is an amine curing agent, an acid anhydride curing agent or a polyol curing agent; the amine curing agent is polyetheramine D230, diethylenetriamine or triethylenetetramine; the acid anhydride curing agent is phthalic anhydride or adipic anhydride; the polyol curing agent is polyether polyol; The organic solvent is N,N-dimethylformamide, glycol ether or phenylethanol; The hydrophobic modifier is heptadecafluorosilane, fatty acid or alkyl silane coupling agent; The mass ratio of epoxy resin, curing agent, organic solvent and hydrophobic modifier is 5:1-3:15-45:0.05-0.
15.
9. The preparation method according to claim 1 or 8, It is characterized in that The heating temperature is 90-110° C. and the heating time is 0.5-1.5 h.
10. The shape memory photothermal anti-icing superhydrophobic material obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Photo-thermal response self-healing coating and preparation method thereof
CN119842290A