High-temperature-resistant diaphragm composite material for lithium battery and preparation method thereof
By using high-density polyethylene, compatibilizers and additives in lithium-ion battery separators, the problem of poor stability of lithium-ion battery separators at high temperatures is solved, and the high temperature and mechanical properties of the material are significantly improved, avoiding the need for avoiding the Battery short circuit and thermal runaway accidents.
Patent Information
- Application Number
- CN202411197914.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium-ion battery separators have poor stability at high temperatures, which can easily lead to short circuits and thermal runaway inside the battery, affecting performance and safety.
Using a preparation method of high-temperature resistant membrane composite material for lithium batteries, the melt extrusion process of high-density polyethylene, compatible agent, additive, lubricant and antioxidant at a specific temperature is prepared to improve compatibility. and materials that enhance mechanical properties. Compatible agents increase isocyanate groups through graft polymerization, and additives entangle with high-density polyethylene molecular chains through branched molecular chains to improve cross-linking density and material stability.
It significantly improves the high temperature resistance and mechanical properties of the material, reduces the shrinkage rate and puncture strength, enhances the stability of the diaphragm, and avoids battery short circuit and thermal runaway accidents at high temperatures.
Smart Images

Figure CN119060434A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of materials, and in particular to a high temperature resistant diaphragm composite material for a lithium battery and a preparation method thereof. Background Art
[0002] In the context of the rapid development of modern industrial society, the consumption of non-renewable energy such as oil and natural gas has increased year by year, which has not only led to a large reduction in fossil energy reserves and caused an energy crisis, but also seriously polluted the environment, exacerbated the greenhouse effect and climate warming. Therefore, the use of clean energy such as electricity to replace fossil energy has become a key research topic. Since the storage and conversion of electrical energy requires energy storage and conversion devices, among various types of energy storage and conversion devices, lithium-ion batteries have occupied a dominant position in the energy storage system market with their high energy density and long cycle life.
[0003] At present, the components of lithium-ion batteries are mainly electrode materials, diaphragms and electrolytes. The main function of the diaphragm is to prevent direct contact between the positive and negative electrodes of the battery and to promote the shuttling of lithium ions between the positive and negative electrodes. At present, commercial diaphragms are mainly polyolefin diaphragms represented by polyethylene. This type of diaphragm has the advantages of low production cost and uniform pore structure. However, the defects are also very obvious. The most serious problem is that the high-temperature stability of polyolefin diaphragms is poor. When heated, they will shrink, causing internal short circuits in the battery, which will not only affect the performance of the battery, but also cause safety accidents such as thermal runaway. Therefore, it is urgent to improve the high-temperature resistance of polyethylene diaphragm materials. Summary of the invention
[0004] 1. Technical issues to be solved
[0005] In view of the deficiencies in the prior art, the present invention provides a high temperature resistant diaphragm composite material for a lithium battery and a preparation method thereof.
[0006] (II) Technical solution
[0007] A method for preparing a high temperature resistant diaphragm composite material for a lithium battery, the composite material comprising the following raw materials in parts by weight:
[0008]
[0009] The preparation method comprises the following steps:
[0010] The first step is to mix high-density polyethylene, compatibilizer, additive, lubricant and antioxidant in a mixer, and set the mixing temperature to 120-150° C. to obtain a precursor material;
[0011] The second step is to feed the precursor material into the main feeding hopper of the twin-screw extruder through the feeding hopper, control the temperature of the extrusion conveying section to 160-180°C, the temperature of the melting section to 180-200°C, and the temperature of the homogenizing section to 200-220°C, and carry out the melt extrusion process.
[0012] As a further embodiment of the present invention, the preparation method of the compatibilizer is as follows:
[0013] SEBS, 3-isopropyl-dimethylbenzyl isocyanate and initiator benzoyl peroxide are placed in a torque rheometer, and then the temperature is controlled to 180-200°C, and the screw speed is adjusted to 40-50rpm. After melt grafting for 5-10 minutes, the temperature is lowered and the material is discharged to obtain a compatibilizer.
[0014] In the above technical solution, 3-isopropyl-dimethylbenzyl isocyanate is used as a grafting agent, and under the action of an initiator, graft polymerization is carried out on the thermoplastic elastomer SEBS to obtain a SEBS derivative containing an isocyanate active substituent in its structure, namely a compatibilizer.
[0015] As a further embodiment of the present invention, the preparation method of the additive is as follows:
[0016] Add modified polyethersulfone and N,N-dimethylformamide into a reactor filled with nitrogen, stir mechanically to mix evenly, and then add 1,2,3,4-tetrahydro-1,4-methylnaphthalene-5,8-diol and a catalyst into the reactor. After the addition, gradually increase the temperature to 70-80°C, stir continuously for 6-9 hours, evaporate and remove the solvent, collect the solid product, and obtain the additive through post-treatment.
[0017] As a further embodiment of the present invention, the preparation method of the modified polyether sulfone is as follows:
[0018] Add polyethersulfone to dimethyl sulfoxide and start stirring. After a uniform mixed solution is formed, add epichlorohydrin to the mixed solution and add a tin catalyst at the same time. After the addition is completed, gradually increase the temperature to 60-70°C, stir and react for 8-16 hours, evaporate and remove the solvent, collect the solid material, wash and vacuum dry it, and then obtain modified polyethersulfone.
[0019] As a further embodiment of the present invention, the number average molecular weight of the polyethersulfone is 6,000.
[0020] As a further embodiment of the present invention, the mass ratio of the polyethersulfone to epichlorohydrin is 1:0.1-0.15.
[0021] As a further embodiment of the present invention, the tin catalyst is tin chloride.
[0022] As a further embodiment of the present invention, the catalyst is boron trifluoride etherate complex, and the mass of the boron trifluoride etherate complex added is 3-5% of the total mass of the modified polyethersulfone and 1,2,3,4-tetrahydro-1,4-methylnaphthalene-5,8-diol.
[0023] In the above technical scheme, first, under the action of a tin catalyst, epichlorohydrin is used as a modifier to carry out a Friedel-Crafts alkylation reaction with polyethersulfone to obtain a polyethersulfone modified product containing an epoxy substituent in the structure, namely, modified polyethersulfone, and then, using the catalysis of a boron trifluoride ether complex, it is continuously subjected to ring-opening addition with the active substituted hydroxyl groups in the structure of 1,2,3,4-tetrahydro-1,4-methylnaphthalene-5,8-diol, thereby obtaining a polyethersulfone polymer having a branched block alternating structure, namely, an additive.
[0024] As a further embodiment of the present invention, the lubricant is polyethylene wax; and the antioxidant is any one of hindered phenol antioxidants.
[0025] A high temperature resistant diaphragm composite material for lithium battery is prepared by the above preparation method.
[0026] (III) Beneficial technical effects
[0027] (1) The compatibilizer prepared by the present invention is SEBS containing an isocyanate active substituent in its structure, wherein the isocyanate group can interact with the hydroxyl group generated by the ring-opening addition reaction in the additive structure during the subsequent high-temperature melting process, so that the branched molecular chain of the additive can be entangled with the high-density polyethylene molecular chain, thereby improving the compatibility between the additive and the high-density polyethylene matrix. In addition, the thermoplastic elastomer SEBS can produce a good toughening effect on high-density polyethylene, which is beneficial to improving the mechanical properties of the material.
[0028] (2) The present invention allows the branched molecular chains of the additive to be entangled with the high-density polyethylene molecular chains under the action of the compatibilizer. On the one hand, this entangled molecular chain structure can greatly increase the cross-linking density of the high-density polyethylene molecular chains, resulting in relatively difficult movement of the high-density polyethylene molecular chains, thereby effectively improving the high-temperature resistance of the material. In addition, the benzonorbornene heterocyclic structure and continuous benzene ring structure contained in the additive molecular chain are rigid, and after entering the high-density polyethylene molecular chain, the material can exhibit higher stability, thereby further enhancing the high-temperature resistance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0030] Figure 1 This is the infrared analysis test chart of the additive. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0032] Preparation Example 1
[0033] Preparation of compatibilizer:
[0034] 10g of SEBS, 4.5g of 3-isopropyl-dimethylbenzyl isocyanate and 0.1g of initiator benzoyl peroxide were placed in a torque rheometer, and then the temperature was controlled to 180°C, and the screw speed was adjusted to 50rpm. After melt grafting for 10 minutes, the temperature was lowered and the material was discharged to obtain a compatibilizer.
[0035] 0.5 g of the compatibilizer was weighed as a sample, and a hydrochloric acid-di-n-butylamine titration method was used to perform a titration test on the sample. The test result showed that the percentage of isocyanate groups in the sample was 6.71%.
[0036] Preparation Example 2
[0037] Preparation of additives:
[0038] Step A, adding 1.5 g of polyethersulfone with a number average molecular weight of 6000 to dimethyl sulfoxide, starting stirring, and after a uniform mixed solution is formed, adding 0.2 g of epichlorohydrin to the mixed solution, and adding tin chloride at the same time, after the addition is complete, gradually raising the temperature to 65° C., stirring and reacting for 12 hours, evaporating and removing the solvent, collecting the solid material, washing, and vacuum drying to obtain the modified polyethersulfone;
[0039] Step B, add 2.4g of modified polyethersulfone and N,N-dimethylformamide to a reactor filled with nitrogen, stir mechanically to mix evenly, and after forming a uniform liquid, add 0.5g of 1,2,3,4-tetrahydro-1,4-methylnaphthalene-5,8-diol and 0.1g of boron trifluoride ether complex to the reactor. After the addition, gradually increase the temperature to 75°C, stir continuously for 8h, evaporate and remove the solvent, collect the solid product, and obtain the additive through a post-treatment process.
[0040] The additive was made into potassium bromide tablets and subjected to infrared analysis test. The results were as follows Figure 1 As shown, 3292cm -1 The characteristic stretching vibration absorption peak of hydroxyl group appears at 3000~3100cm -1 The characteristic stretching vibration absorption peak of CH of the benzene ring skeleton appeared at 1301cm -1 1171cm -1 The characteristic stretching vibration absorption peak of sulfone group S=O appeared at 1059cm -1 The characteristic stretching vibration absorption peak of ether bond appears at .
[0041] Example 1
[0042] A high temperature resistant diaphragm composite material for lithium battery, comprising the following raw materials in parts by weight:
[0043]
[0044] The preparation method of the composite material comprises the following steps:
[0045] The first step is to mix high-density polyethylene, compatibilizer, additive, lubricant and antioxidant 1010 in a mixer, and set the mixing temperature to 120° C. to obtain a precursor material;
[0046] The second step is to feed the precursor material into the main feeding hopper of the twin-screw extruder through the feeding hopper, control the temperature of the extrusion conveying section to 160°C, the temperature of the melting section to 180°C, and the temperature of the homogenizing section to 200°C, and carry out the melt extrusion process.
[0047] The preparation method of the compatibilizer is shown in Preparation Example 1, and the preparation method of the additive is shown in Preparation Example 2. The following examples and comparative examples are the same.
[0048] Example 2
[0049] A high temperature resistant diaphragm composite material for lithium battery, comprising the following raw materials in parts by weight:
[0050]
[0051] The preparation method of the composite material comprises the following steps:
[0052] The first step is to mix high-density polyethylene, compatibilizer, additive, lubricant and antioxidant 1010 in a mixer, and set the mixing temperature to 130° C. to obtain a precursor material;
[0053] The second step is to feed the precursor material into the main feeding hopper of the twin-screw extruder through the feeding hopper, control the temperature of the extrusion conveying section to 170°C, the temperature of the melting section to 190°C, and the temperature of the homogenizing section to 210°C, and carry out the melt extrusion process.
[0054] Example 3
[0055] A high temperature resistant diaphragm composite material for lithium battery, comprising the following raw materials in parts by weight:
[0056]
[0057]
[0058] The preparation method of the composite material comprises the following steps:
[0059] The first step is to mix high-density polyethylene, compatibilizer, additive, lubricant and antioxidant 1010 in a mixer, and set the mixing temperature to 150° C. to obtain a precursor material;
[0060] The second step is to feed the precursor material into the main feeding hopper of the twin-screw extruder through the feeding hopper, control the temperature of the extrusion conveying section to 180°C, the temperature of the melting section to 200°C, and the temperature of the homogenizing section to 220°C, and carry out the melt extrusion process.
[0061] Comparative Example 1
[0062] A high temperature resistant diaphragm composite material for lithium battery, comprising the following raw materials in parts by weight:
[0063]
[0064] The preparation method of the composite material comprises the following steps:
[0065] The first step is to mix high-density polyethylene, maleic anhydride grafted polyethylene, additives, lubricants and antioxidants 1010 in a mixer, and set the mixing temperature to 130° C. to obtain a precursor material;
[0066] The second step is to feed the precursor material into the main feeding hopper of the twin-screw extruder through the feeding hopper, control the temperature of the extrusion conveying section to 170°C, the temperature of the melting section to 190°C, and the temperature of the homogenizing section to 210°C, and carry out the melt extrusion process.
[0067] Comparative Example 2
[0068] A high temperature resistant diaphragm composite material for lithium battery, comprising the following raw materials in parts by weight:
[0069]
[0070]
[0071] The preparation method of the composite material comprises the following steps:
[0072] The first step is to mix high-density polyethylene, additives, lubricants and antioxidants 1010 in a mixer, and set the mixing temperature to 130° C. to obtain a precursor material;
[0073] The second step is to feed the precursor material into the main feeding hopper of the twin-screw extruder through the feeding hopper, control the temperature of the extrusion conveying section to 170°C, the temperature of the melting section to 190°C, and the temperature of the homogenizing section to 210°C, and carry out the melt extrusion process.
[0074] Comparative Example 3
[0075] A high temperature resistant diaphragm composite material for lithium battery, comprising the following raw materials in parts by weight:
[0076]
[0077] The preparation method of the composite material comprises the following steps:
[0078] The first step is to mix high-density polyethylene, compatibilizer, lubricant and antioxidant 1010 in a mixer, and set the mixing temperature to 130° C. to obtain a precursor material;
[0079] The second step is to feed the precursor material into the main feeding hopper of the twin-screw extruder through the feeding hopper, control the temperature of the extrusion conveying section to 170°C, the temperature of the melting section to 190°C, and the temperature of the homogenizing section to 210°C, and carry out the melt extrusion process.
[0080] Test Case
[0081] The composite materials in the above examples and comparative examples were tested for comprehensive properties, and the results are shown in the following table:
[0082]
[0083] The test method for tensile strength refers to the standard GB / T 1040.3-2006; the test method for puncture strength refers to the standard GB / T 2679.7-2005; the test method for shrinkage is specifically as follows: the composite material is made into a sample with a specification of 10cm×10cm×2mm, and it is clamped between two clean glass plates, and then placed in a temperature environment of 120°C for 2h, taken out, and the transverse and longitudinal lengths of the diaphragm are measured, and the shrinkage is calculated. The shrinkage calculation formula is [(initial length-length after treatment) / initial length]×100%.
[0084] By analyzing the test results, it can be seen that the composite material prepared by adding the compatibilizer in Preparation Example 1 of the present invention and the additive prepared in Preparation Example 2 has excellent mechanical properties and high temperature resistance.
[0085] After the compatibilizer was replaced with a conventional maleic anhydride grafted polyethylene compatibilizer, the toughening effect of SEBS was lost, and it can be clearly seen that the mechanical properties decreased. After the compatibilizer was directly removed, the additive molecular chain could not be entangled with the high-density polyethylene molecular chain, resulting in a decrease in cross-linking density and a further decrease in the mechanical properties of the material, especially the puncture strength, which decreased significantly. As the cross-linking density decreased, the movement of the molecular chain was less hindered, so the high temperature resistance was also negatively affected.
[0086] After removing the additives, the high temperature resistance and mechanical properties of the material are both severely negatively affected. This is also due to the reduction of the cross-linking density of the high-density polyethylene molecular chain and the decrease in the density of the material.
[0087] Based on the ideal embodiment of the present invention, through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing a high temperature resistant diaphragm composite material for a lithium battery, characterized in that: The composite material comprises the following raw materials in parts by weight: The preparation method comprises the following steps: The first step is to mix high-density polyethylene, compatibilizer, additive, lubricant and antioxidant in a mixer, and set the mixing temperature to 120-150° C. to obtain a precursor material; The second step is to feed the precursor material into the main feeding hopper of the twin-screw extruder through the feeding hopper, control the temperature of the extrusion conveying section to 160-180°C, the temperature of the melting section to 180-200°C, and the temperature of the homogenizing section to 200-220°C, and carry out the melt extrusion process.
2. The method for preparing a high temperature resistant diaphragm composite material for a lithium battery according to claim 1, characterized in that: The preparation method of the compatibilizer is as follows: SEBS, 3-isopropyl-dimethylbenzyl isocyanate and initiator benzoyl peroxide are placed in a torque rheometer, and then the temperature is controlled to 180-200°C, and the screw speed is adjusted to 40-50rpm. After melt grafting for 5-10 minutes, the temperature is lowered and the material is discharged to obtain a compatibilizer.
3. The method for preparing a high temperature resistant diaphragm composite material for a lithium battery according to claim 1, characterized in that: The preparation method of the additive is as follows: Add modified polyethersulfone and N,N-dimethylformamide into a reactor filled with nitrogen, stir mechanically to mix evenly, and then add 1,2,3,4-tetrahydro-1,4-methylnaphthalene-5,8-diol and a catalyst into the reactor. After the addition, gradually increase the temperature to 70-80°C, stir continuously for 6-9 hours, evaporate and remove the solvent, collect the solid product, and obtain the additive through post-treatment.
4. The method for preparing a high temperature resistant diaphragm composite material for a lithium battery according to claim 3, characterized in that: The preparation method of the modified polyether sulfone is as follows: Add polyethersulfone to dimethyl sulfoxide and start stirring. After a uniform mixed solution is formed, add epichlorohydrin to the mixed solution and add a tin catalyst at the same time. After the addition is completed, gradually increase the temperature to 60-70°C, stir and react for 8-16 hours, evaporate and remove the solvent, collect the solid material, wash and vacuum dry it, and then obtain modified polyethersulfone.
5. The method for preparing a high temperature resistant diaphragm composite material for a lithium battery according to claim 4, characterized in that: The number average molecular weight of the polyethersulfone is 6,000.
6. The method for preparing a high temperature resistant diaphragm composite material for a lithium battery according to claim 4, characterized in that: The mass ratio of the polyethersulfone to epichlorohydrin is 1:0.1-0.
15.
7. The method for preparing a high temperature resistant diaphragm composite material for a lithium battery according to claim 4, characterized in that: The tin catalyst is tin chloride.
8. The method for preparing a high temperature resistant diaphragm composite material for a lithium battery according to claim 3, characterized in that: The catalyst is a boron trifluoride ether complex, and the mass of the boron trifluoride ether complex added is 3-5% of the total mass of the modified polyether sulfone and 1,2,3,4-tetrahydro-1,4-methylnaphthalene-5,8-diol.
9. The method for preparing a high temperature resistant diaphragm composite material for a lithium battery according to claim 1, characterized in that: The lubricant is polyethylene wax; and the antioxidant is any one of hindered phenol antioxidants.
10. A high temperature resistant diaphragm composite material for lithium battery, characterized in that: The method is prepared according to claim 1.