Rice hull ash-containing silicon dioxide comprehensive material and preparation method thereof
By blending the rice husk ash silica with quaternized maleimide copolymer and other components, a cross-linking network is formed, which solves the problem of insufficient performance of rice husk ash silica material and achieves high material Improved stretching, flame retardant and antibacterial effects.
Patent Information
- Application Number
- CN202411407117.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The flame retardant, antibacterial and tensile properties of existing rice husk ash silica materials are insufficient, which limits its application range.
The components such as rice husk ash silica, quaternized maleimide copolymer, epoxy phenylphosphorus oxide, polyethylene resin and maleic anhydride grafted polyethylene are mixed through a twin-screw extruder. Prepare to form a comprehensive material containing rice husk ash silica, and improve the compatibility and performance of the material through open ring reaction and crosslinking network.
The tensile performance, flame retardant performance and antibacterial effect of the material are significantly improved, forming a material with superior comprehensive performance.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, in particular to a comprehensive material containing rice husk ash and silicon dioxide and a preparation method thereof. Background Art
[0002] Rice husk ash silica is a green, renewable industrial raw material extracted from rice husks. It has broad application prospects and unique physical and chemical properties. Therefore, applying it to materials is expected to improve the comprehensive performance of the materials. For example, patent CN110172180B inorganic fiber / silicon dioxide nanomaterials and preparation methods and applications thereof, this invention uses in-situ growth of silicon dioxide on inorganic fibers to form nanomaterials, which is easy to operate and low in cost. For example, patent CN1017349.3A nano-silicon dioxide insulation material and preparation method thereof, this invention has good insulation performance and low preparation cost. In summary, its flame retardant and antibacterial effects have not been improved, which greatly limits its application. Summary of the invention
[0003] 1. Technical issues to be resolved In view of the deficiencies in the prior art, the present invention provides a rice husk ash-containing silica comprehensive material and a preparation method thereof, which has good flame retardant, tensile and antibacterial effects.
[0004] (II) Technical solution To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a comprehensive material containing rice husk ash silica, comprising the following weight components: 5-10 weight parts of rice husk ash silica, 12-18 weight parts of quaternized maleimide copolymer, 5-10 weight parts of epoxyphenyl phosphorus oxide, 20-40 weight parts of polyethylene resin, and 10-15 weight parts of maleic anhydride grafted polyethylene.
[0005] Preferably, the preparation method of the quaternized maleimide copolymer is: (1) Adding 2,5-divinyl-1,4-benzenedicarboxaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to a toluene solvent, stirring and mixing, and reflux reaction at 110-130° C. for 5-10 hours. After the reaction is completed, filtering and drying to obtain olefinated phenylphosphine oxide; (2) Add olefinated phenylphosphine oxide and 3-(dimethylamino)-1-propanethiol to a reaction vessel containing N,N-dimethylformamide, introduce nitrogen protection, then add benzoin dimethyl ether catalyst, and irradiate the reaction vessel under ultraviolet light for 2-4 hours. The ultraviolet light has a wavelength of 365nm and a power of 60W. After the reaction, distill under reduced pressure, recrystallize the product with toluene, and wash to obtain intermediate 1; (3) Dissolve 6-maleimidocaproic acid in 1,4-dioxane solvent and stir evenly, then add 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid, continue stirring for 2-4 minutes, then evacuate the system for 10-12 minutes, stir in an oil bath at 70-85°C in the dark for 22-25 hours, after which the product is precipitated in water, centrifuged at 8000-8100 rpm for 4-6 minutes, washed with deionized water 2-4 times, and dried in vacuum to obtain intermediate 2; (4) Add 10-16 parts by weight of intermediate 1 and 8-15 parts by weight of intermediate 2 to N,N-dimethylformamide solvent, stir to dissolve, carry out quaternization reaction at 75-90° C. for 4-8 hours, and then perform rotary distillation, wash and dry to obtain a quaternized maleimide copolymer.
[0006] Preferably, the mass ratio of 2,5-divinyl-1,4-benzenedicarbaldehyde to 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in (1) is 1:2.1-2.6.
[0007] Preferably, the mass ratio of olefinated phenylphosphine oxide, 3-(dimethylamino)-1-propanethiol, and benzoin dimethyl ether catalyst in (2) is 1:1.2-1.5:0.01-0.03.
[0008] Preferably, the mass ratio of 6-maleimidocaproic acid, 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid in (3) is 1:1.1-1.4:0.02-0.03:0.01-0.02.
[0009] Preferably, the preparation method of the epoxyphenyl phosphorus oxide is: 11-15 parts by weight of intermediate 1 and 18-22 parts by weight of epichlorohydrin are added to a reactor filled with N,N-dimethylformamide, stirred for 10-15 minutes, reacted at 55-70° C. for 6-10 hours, distilled after completion, washed with petroleum ether, and obtained epoxyphenyl phosphorus oxide.
[0010] Preferably, the preparation method of the comprehensive material containing rice husk ash silica is: adding rice husk ash silica, quaternized maleimide copolymer, epoxyphenyl phosphorus oxide, polyethylene resin, and maleic anhydride grafted polyethylene into a twin-screw extruder, with a blending temperature of 180-190°C and an extrusion temperature of 170-180°C to obtain the comprehensive material containing rice husk ash silica.
[0011] 3. Beneficial technical effects The invention obtains a comprehensive material containing rice husk ash silica by adding rice husk ash silica, quaternized maleimide copolymer, epoxyphenyl phosphorus oxide, polyethylene resin and maleic anhydride grafted polyethylene into a twin-screw extruder, blending and extruding.
[0012] During the blending process, the hydroxyl group and carboxyl group in the quaternized maleimide copolymer will undergo a ring-opening reaction with the epoxy group in the epoxyphenyl phosphorus oxide to generate hydroxyl groups that further react with the anhydride in the maleic anhydride grafted polyethylene, thereby increasing the compatibility between each other and the polyethylene resin. A tight cross-linking network will be formed between the three, which will disperse to various cross-linking points when subjected to external force, thereby unloading the force and improving the tensile properties of the material; the phosphorus and sulfur elements contained in the comprehensive material containing rice husk ash silica have good flame retardancy, and the rice husk ash silica itself also has good flame retardancy, together forming a flame retardant system; the comprehensive material containing rice husk ash silica contains a large amount of quaternary ammonium salt groups, which has a good antibacterial effect. DETAILED DESCRIPTION
[0013] Example 1 (1) adding 2,5-divinyl-1,4-benzenedicarboxaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to a toluene solvent, wherein the mass ratio of 2,5-divinyl-1,4-benzenedicarboxaldehyde to 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1:2.1, stirring and mixing, and reflux reaction at 110° C. for 5 hours. After the reaction is completed, filtering and drying to obtain olefinated phenylphosphine oxide; (2) Add olefinated phenylphosphine oxide and 3-(dimethylamino)-1-propanethiol to a reaction vessel containing N,N-dimethylformamide, introduce nitrogen for protection, and then add benzoin dimethyl ether catalyst, wherein the mass ratio of olefinated phenylphosphine oxide, 3-(dimethylamino)-1-propanethiol and benzoin dimethyl ether catalyst is 1:1.2:0.01, irradiate the reaction vessel under ultraviolet light for 2 hours, and then distill under reduced pressure after the reaction ends. The product is recrystallized with toluene and washed to obtain intermediate 1; (3) Dissolve 6-maleimidocaproic acid in 1,4-dioxane solvent and stir evenly, then add 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid, wherein the mass ratio of 6-maleimidocaproic acid, 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid is 1:1.1:0.02:0.01, continue stirring for 2 min, then evacuate the system for 10 min, stir in a 70°C oil bath in the dark for 22 h, after which the product is precipitated in water, centrifuged at 8000 rpm for 4 min, washed twice with deionized water, and dried in vacuum to obtain intermediate 2; (4) adding 10 parts by weight of intermediate 1 and 8 parts by weight of intermediate 2 to N,N-dimethylformamide solvent, stirring to dissolve, and carrying out quaternization reaction at 75° C. for 4 hours. After completion, rotary distillation is performed, and the reaction is washed and dried to obtain a quaternized maleimide copolymer; (5) 11 parts by weight of intermediate 1 and 18 parts by weight of epichlorohydrin were added to a reactor containing N,N-dimethylformamide, stirred for 10 minutes, reacted at 55° C. for 6 hours, and then distilled and washed with petroleum ether to obtain epoxyphenylphosphine oxide; (6) Add 5 parts by weight of rice husk ash silica, 12 parts by weight of quaternized maleimide copolymer, 5 parts by weight of epoxyphenyl phosphine oxide, 20 parts by weight of polyethylene resin, and 10 parts by weight of maleic anhydride grafted polyethylene into a twin-screw extruder at a blending temperature of 180° C. and an extrusion temperature of 170° C. to obtain a comprehensive material containing rice husk ash silica.
[0014] Example 2 (1) adding 2,5-divinyl-1,4-benzenedicarboxaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to a toluene solvent, wherein the mass ratio of 2,5-divinyl-1,4-benzenedicarboxaldehyde to 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1:2.6, stirring and mixing, and reflux reaction at 130° C. for 10 hours. After the reaction is completed, filtering and drying to obtain olefinated phenylphosphine oxide; (2) Add olefinated phenylphosphine oxide and 3-(dimethylamino)-1-propanethiol to a reaction vessel filled with N,N-dimethylformamide, introduce nitrogen for protection, and then add benzoin dimethyl ether catalyst, wherein the mass ratio of olefinated phenylphosphine oxide, 3-(dimethylamino)-1-propanethiol and benzoin dimethyl ether catalyst is 1:1.5:0.03, irradiate the reaction vessel under ultraviolet light for 4 hours, and then distill under reduced pressure after the reaction ends. The product is recrystallized with toluene and washed to obtain intermediate 1; (3) Dissolve 6-maleimidocaproic acid in 1,4-dioxane solvent and stir evenly, then add 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid, wherein the mass ratio of 6-maleimidocaproic acid, 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid is 1:1.4:0.03:0.02, continue stirring for 4 min, then evacuate the system for 12 min, stir in an oil bath at 85 °C in the dark for 25 h, after which the product is precipitated in water, centrifuged at 8100 rpm for 6 min, washed 4 times with deionized water, and dried in vacuum to obtain intermediate 2; (4) Add 16 parts by weight of intermediate 1 and 15 parts by weight of intermediate 2 to N,N-dimethylformamide solvent, stir to dissolve, and carry out quaternization reaction at 90° C. for 8 hours. After the reaction, perform rotary distillation, wash and dry to obtain a quaternized maleimide copolymer; (5) Add 15 parts by weight of intermediate 1 and 22 parts by weight of epichlorohydrin into a reactor filled with N,N-dimethylformamide, stir for 15 minutes, react at 70° C. for 10 hours, distill after reaction, and wash with petroleum ether to obtain epoxyphenylphosphorus oxide; (6) 10 parts by weight of rice husk ash silica, 18 parts by weight of quaternized maleimide copolymer, 10 parts by weight of epoxyphenyl phosphine oxide, 40 parts by weight of polyethylene resin, and 15 parts by weight of maleic anhydride grafted polyethylene are added into a twin-screw extruder at a blending temperature of 190° C. and an extrusion temperature of 180° C. to obtain a comprehensive material containing rice husk ash silica.
[0015] Example 3 (1) adding 2,5-divinyl-1,4-benzenedicarboxaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to a toluene solvent, wherein the mass ratio of 2,5-divinyl-1,4-benzenedicarboxaldehyde to 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1:2.35, stirring and mixing, and reflux reaction at 120° C. for 7.5 hours. After the reaction is completed, filtering and drying to obtain olefinated phenylphosphine oxide; (2) Add olefinated phenylphosphine oxide and 3-(dimethylamino)-1-propanethiol to a reaction vessel containing N,N-dimethylformamide, introduce nitrogen for protection, and then add benzoin dimethyl ether catalyst, wherein the mass ratio of olefinated phenylphosphine oxide, 3-(dimethylamino)-1-propanethiol and benzoin dimethyl ether catalyst is 1:1.35:0.02, irradiate the reaction vessel under ultraviolet light for 3 hours, and then distill under reduced pressure after the reaction ends. The product is recrystallized with toluene and washed to obtain intermediate 1; (3) Dissolve 6-maleimidocaproic acid in 1,4-dioxane solvent and stir evenly, then add 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid, wherein the mass ratio of 6-maleimidocaproic acid, 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid is 1:1.25:0.025:0.015, continue stirring for 3 min, then evacuate the system for 11 min, stir in an oil bath at 77 °C in the dark for 24 h, after which the product is precipitated in water, centrifuged at 8050 rpm for 5 min, washed three times with deionized water, and dried in vacuum to obtain intermediate 2; (4) adding 13 parts by weight of intermediate 1 and 11.5 parts by weight of intermediate 2 to N,N-dimethylformamide solvent, stirring to dissolve, and carrying out quaternization reaction at 85° C. for 6 hours. After completion, rotary distillation is performed, and the reaction is washed and dried to obtain a quaternized maleimide copolymer; (5) 13 parts by weight of intermediate 1 and 20 parts by weight of epichlorohydrin were added to a reactor containing N,N-dimethylformamide, stirred for 12.5 minutes, reacted at 60° C. for 8 hours, and then distilled and washed with petroleum ether to obtain epoxyphenylphosphorus oxide; (6) 7.5 parts by weight of rice husk ash silica, 16 parts by weight of quaternized maleimide copolymer, 7.5 parts by weight of epoxyphenyl phosphine oxide, 30 parts by weight of polyethylene resin, and 12.5 parts by weight of maleic anhydride grafted polyethylene are added into a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 175° C. to obtain a comprehensive material containing rice husk ash silica.
[0016] Comparative Example 1 This comparative example is different from Example 3 in that no quaternized maleimide copolymer is added.
[0017] Comparative Example 2 This comparative example is compared with Example 3, except that no epoxyphenylphosphine oxide is added.
[0018] The tensile properties of the composite material containing rice husk ash and silica were tested by a universal material testing machine. The test results are shown in Table 1.
[0019] Table 1: Tensile properties tested.
[0020] project Tensile strength (MPa) Example 1 63.5 Example 2 65.7 Example 3 63.1 Comparative Example 1 51.2 Comparative Example 2 43.6 It can be seen from Table 1 that Examples 1-3 of the present invention have better tensile properties than Comparative Examples 1-2.
[0021] The oxygen index was determined according to the method specified in GB / T2406-2008. The flame retardant grade was tested according to UL94-2009 standard. FV-0: the burning time does not exceed 10 seconds and does not ignite the absorbent cotton. FV-1: the burning time does not exceed 30 seconds and does not ignite the absorbent cotton. FV-2: the burning time does not exceed 30 seconds and ignites the absorbent cotton. The test results are shown in Table 2.
[0022] Table 2: Flame retardancy tests.
[0023] project Limiting oxygen index (%) Vertical burning level Example 1 32.4 FV-0 Example 2 33.5 FV-0 Example 3 32.6 FV-0 Comparative Example 1 17.5 FV-1 Comparative Example 2 16.8 FV-1 It can be seen from Table 2 that Examples 1-3 of the present invention have better flame retardant properties than Comparative Examples 1-2.
[0024] Pipette 1 mL of 10 8 CFU / mL of Staphylococcus aureus was added to PBS buffer, and then diluted 10-fold to 10 5 CFU / mL, then add the samples (1 cm×1 cm×0.2 cm) of Example 1-3 and Comparative Example 1-2, and then culture them in a constant temperature incubator at 37°C with shaking for 24 h. After culture, add PBS buffer to dilute the bacterial solution 10 times in sequence, then transfer 0.5 mL of the bacterial solution to inoculate into the agar medium, and continue to culture them at 37°C with shaking for 24 h. After culture, count the colonies and count the antibacterial rate. The test results are shown in Table 3.
[0025] Table 3: Antimicrobial testing.
[0026] project Antibacterial rate (%) Example 1 99.7 Example 2 99.8 Example 3 99.8 Comparative Example 1 53.4 Comparative Example 2 48.7 It can be seen from Table 3 that the rice husk ash-containing silica comprehensive material Examples 1-3 of the present invention have better antibacterial effects than Comparative Examples 1-2.
[0027] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A rice husk ash-containing silica comprehensive material, characterized in that: The invention comprises the following components by weight: 5-10 parts by weight of rice husk ash silica, 12-18 parts by weight of quaternized maleimide copolymer, 5-10 parts by weight of epoxyphenyl phosphorus oxide, 20-40 parts by weight of polyethylene resin and 10-15 parts by weight of maleic anhydride grafted polyethylene.
2. The rice husk ash-containing silica comprehensive material according to claim 1, characterized in that: The preparation method of the quaternized maleimide copolymer is: (1) Adding 2,5-divinyl-1,4-benzenedicarboxaldehyde and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to a toluene solvent, stirring and mixing, and reflux reaction at 110-130° C. for 5-10 hours. After the reaction is completed, filtering and drying to obtain olefinated phenylphosphine oxide; (2) Add olefinated phenylphosphine oxide and 3-(dimethylamino)-1-propanethiol to a reaction vessel containing N,N-dimethylformamide, introduce nitrogen protection, then add benzoin dimethyl ether catalyst, irradiate the reaction vessel under ultraviolet light for 2-4 hours, and then distill under reduced pressure after the reaction. The product is recrystallized with toluene and washed to obtain intermediate 1; (3) Dissolve 6-maleimidocaproic acid in 1,4-dioxane solvent and stir evenly, then add 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid, continue stirring for 2-4 minutes, then evacuate the system for 10-12 minutes, stir in an oil bath at 70-85°C in the dark for 22-25 hours, after which the product is precipitated in water, centrifuged at 8000-8100 rpm for 4-6 minutes, washed with deionized water 2-4 times, and dried in vacuum to obtain intermediate 2; (4) Add 10-16 parts by weight of intermediate 1 and 8-15 parts by weight of intermediate 2 to N,N-dimethylformamide solvent, stir to dissolve, carry out quaternization reaction at 75-90° C. for 4-8 hours, and then perform rotary distillation, wash and dry to obtain a quaternized maleimide copolymer.
3. The rice husk ash-containing silica comprehensive material according to claim 2, characterized in that: The mass ratio of 2,5-divinyl-1,4-benzenedicarbaldehyde to 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in (1) is 1:2.1-2.
6.
4. The rice husk ash-containing silica comprehensive material according to claim 2, characterized in that: The mass ratio of olefinated phenylphosphine oxide, 3-(dimethylamino)-1-propanethiol and benzoin dimethyl ether catalyst in (2) is 1:1.2-1.5:0.01-0.
03.
5. The rice husk ash-containing silica comprehensive material according to claim 2, characterized in that: The mass ratio of 6-maleimidocaproic acid, 4-vinylbenzyl chloride, azobisisobutyronitrile and 2-(dodecyltrithiocarbonate)-2-methylpropionic acid in (3) is 1:1.1-1.4:0.02-0.03:0.01-0.
02.
6. The rice husk ash-containing silica comprehensive material according to claim 1, characterized in that: The preparation method of the epoxy phenyl phosphorus oxide is as follows: 11-15 parts by weight of the intermediate 1 and 18-22 parts by weight of epichlorohydrin are added into a reactor filled with N,N-dimethylformamide, stirred for 10-15 minutes, reacted at 55-70° C. for 6-10 hours, distilled after reaction, and washed with petroleum ether to obtain the epoxy phenyl phosphorus oxide.
7. A method for preparing a rice husk ash-containing silica composite material as claimed in any one of claims 1 to 6, characterized in that: The preparation method of the rice husk ash silica-containing comprehensive material is as follows: rice husk ash silica, quaternized maleimide copolymer, epoxyphenyl phosphorus oxide, polyethylene resin, and maleic anhydride grafted polyethylene are added into a twin-screw extruder, the blending temperature is 180-190° C., and the extrusion temperature is 170-180° C., so as to obtain the rice husk ash silica-containing comprehensive material.