Resin composition and manufacturing method thereof

By using copolymers of aromatic monomers and alicyclic monomers, resins with non-polar backbone structures are prepared, and the problems of low glass transfer temperature and insufficient peeling strength of the liquid rubber resin substrate are solved, thereby achieving low dielectric of the substrate Features and performance improvements.

CN119060467APending Publication Date: 2024-12-03NANYA PLASTICS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310879733.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2023-07-18
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When existing liquid rubber resins are used to manufacture substrates, they are prone to have disadvantages such as low glass transfer temperature, poor reactivity, poor processability, and low peel strength, and it is difficult to meet the needs of low dielectric characteristics and performance improvements at the same time.

Method used

Using a copolymer including aromatic monomers and alicyclic monomers, a copolymer with a molecular weight between 2000 and 5000 is prepared by neutralizing the Lewis acid catalyst and alkaline aqueous solution, containing a non-polar backbone structure to improve the Glass transfer temperature and peel strength of the substrate.

Benefits of technology

The substrate has achieved a significant increase in glass transfer temperature and peel strength while having good low dielectric characteristics, reducing dielectric constant and dielectric loss, and improving reactivity, heat resistance and chemical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004344056900000025
    Figure BDA0004344056900000025
  • Figure BDA0004344056900000026
    Figure BDA0004344056900000026
  • Figure BDA0004344056900000051
    Figure BDA0004344056900000051
Patent Text Reader

Abstract

The invention provides a resin composition comprising a copolymer. The copolymer includes an aromatic monomer and an alicyclic monomer. The molecular weight of the copolymer ranges from 2000 to 5000, and the proportion of the alicyclic monomer relative to the copolymer ranges from 1% to 30%. The invention also provides a manufacturing method of the resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition and a method for preparing the same. Background Art

[0002] In order to make the substrate have the function of high-frequency transmission, it is usually required to have low dielectric properties such as low dielectric constant (Dk) and low dielectric dissipation factor (Df). In order to meet these property requirements, liquid rubber resin with excellent dielectric performance is often used.

[0003] However, since liquid rubber resin is a thermoplastic resin with few reactive groups, the substrate manufactured using it is prone to have disadvantages such as low glass transition temperature (Tg), poor reactivity, poor processability, high melt viscosity, and low peel strength. Therefore, it is a challenge to provide a resin composition that can improve the aforementioned disadvantages while providing a substrate with good low dielectric properties. Summary of the invention

[0004] The invention provides a resin composition, and a substrate manufactured by the resin composition can improve the glass transition temperature and peeling strength while having good low dielectric properties.

[0005] A resin composition of the present invention includes a copolymer. The copolymer includes an aromatic monomer and an alicyclic monomer. The molecular weight of the copolymer ranges from 2000 to 5000, and the proportion of the alicyclic monomer relative to the copolymer ranges from 1% to 30%.

[0006] In one embodiment of the present invention, the copolymer includes vinyl groups, and the proportion of the vinyl groups relative to the copolymer is between 10% and 40%.

[0007] In one embodiment of the present invention, the aromatic monomer includes a styrene monomer, and the ratio of the styrene monomer to the copolymer is between 20% and 90%.

[0008] In one embodiment of the present invention, the copolymer has the following general chemical structure: Where R 1 for R 2 At least one selected from the following chemical formulas: R 3 At least one selected from the following chemical formulas:

[0009] And x:y:z is 1:1~10:0.1~5.

[0010] A method for manufacturing a resin composition of the present invention comprises at least the following steps: manufacturing a copolymer comprises the following steps: dissolving at least a Lewis acid catalyst, an aromatic compound and an alicyclic compound in a solvent to form a first solution; and neutralizing the first solution with an alkaline aqueous solution. The copolymer comprises an aromatic monomer and an alicyclic monomer. The molecular weight of the copolymer ranges from 2000 to 5000, and the proportion of the alicyclic monomer relative to the copolymer ranges from 1% to 30%.

[0011] In one embodiment of the present invention, the copolymer has the following general chemical structure: Where R 1 Derived from at least one of the following compounds: divinylbenzene, butadiene; R 2 Derived from at least one of the following compounds: styrene, tetravinylbiphenyl, divinylnaphthalene; R 3 The compound is derived from at least one of the following compounds: acenaphthylene, cyclopentadiene, cyclobutadiene, norbornene, and dicyclopentadiene; and x:y:z is 1:1-10:0.1-5.

[0012] In one embodiment of the present invention, the Lewis acid catalyst comprises SnCl 4 ·H 2 O or BF 3 ·Oet 3 .

[0013] In one embodiment of the present invention, the solvent includes toluene or dimethylformamide.

[0014] In one embodiment of the present invention, the alkaline aqueous solution comprises a sodium bicarbonate aqueous solution.

[0015] In one embodiment of the present invention, the reaction temperature of the neutralization reaction is greater than or equal to 70°C.

[0016] Based on the above, the resin composition of the present invention introduces a copolymer including an aromatic monomer and an alicyclic monomer, and the proportion of the alicyclic monomer is designed accordingly so that the copolymer contains a non-polar backbone structure. Therefore, the substrate (such as a circuit board or a copper foil substrate) manufactured using the same can have good low dielectric properties while improving the glass transition temperature and peel strength.

[0017] In order to make the above features and advantages of the present invention more obvious and easy to understand, embodiments are specifically described in detail below. DETAILED DESCRIPTION

[0018] In the following detailed description, for the purpose of illustration and not limitation, exemplary embodiments that disclose specific details are described to provide a thorough understanding of the various principles of the present invention. However, it will be apparent to one of ordinary skill in the art that, with the benefit of this disclosure, the present invention may be practiced in other embodiments that depart from the specific details disclosed herein. In addition, descriptions of well-known devices, methods, materials, and other specific details may be omitted to avoid obscuring the description of the various principles of the present invention.

[0019] In this article, the range expressed by "a value to another value" is a summary expression method to avoid listing all the values ​​in the range one by one in the specification. Therefore, the description of a specific numerical range covers any value in the numerical range and a smaller numerical range defined by any value in the numerical range, just as the arbitrary value and the smaller numerical range are written in the description text of the specification.

[0020] Unless otherwise specified, the term "between" used in this specification to define a numerical range is intended to cover a range equal to the endpoint value and between the endpoint values. For example, a size range is between a first value and a second value, which means that the size range can cover the first value, the second value and any value between the first value and the second value.

[0021] In this document, non-limiting terms (such as may, could, for example, or other similar terms) mean optional or optional implementation, inclusion, addition, or presence.

[0022] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood or generally understood in the technical field to which the present invention belongs. It will also be understood that terms (such as those defined in commonly used dictionaries) should be interpreted as having a meaning consistent with their meaning in the relevant technical context and should not be interpreted in an idealized or overly formal sense unless explicitly defined as such herein.

[0023] In this embodiment, the resin composition includes a copolymer of an aromatic monomer and an alicyclic monomer, wherein the molecular weight of the copolymer ranges from 2000 to 5000, and the proportion of the alicyclic monomer relative to the copolymer is between 1% and 30%. Accordingly, the resin composition of the present invention introduces a copolymer including an aromatic monomer and an alicyclic monomer, and the proportion of the alicyclic monomer is designed accordingly so that the copolymer contains a non-polar backbone structure, so that the substrate (such as a circuit board or a copper foil substrate) manufactured using the same can have good low dielectric properties while improving the glass transition temperature and peel strength. Here, the molecular weight is, for example, the number average molecular weight.

[0024] Furthermore, since the non-polar backbone structure is not easily polarized in an electric field, the dielectric constant (Dk, 10kz) of the copper foil substrate manufactured by it can be less than 3.1 and the dielectric loss (Df, 10kz) can be less than 0.0014, so the dielectric properties can be greatly reduced, and the glass transition temperature can be greater than 220°C, so it also has an excellent glass transition temperature. In addition, since the aforementioned copolymer contains a reactive double chain, through intermolecular crosslinking, its reactivity, heat resistance, chemical resistance, cold resistance, low-temperature flexibility (improving brittleness and increasing toughness) and / or improving solvent solubility (such as 40% solubility in acetone) can be improved, but the present invention is not limited to this.

[0025] In some embodiments, the copolymer includes vinyl, and the proportion of vinyl relative to the copolymer is between 10% and 40%. For example, the aromatic monomer includes styrene monomer, and the proportion of styrene monomer relative to the copolymer is between 20% and 90%, but the present invention is not limited to this.

[0026] In some embodiments, the copolymer has the following general chemical structure:

[0027]

[0028] Furthermore, R 1 Expressed as R 2 Selected from one of the following chemical formulas:

[0029] R 3 Selected from one of the following chemical formulas:

[0030] Here, the specific implementation of the copolymer can be any combination of the above, and is not limited to these combinations. As long as the copolymer has a non-polar backbone structure, it belongs to the protection scope of the present invention.

[0031] In addition, x:y:z (molar ratio) is 1:1-10:0.1-5, for example, x:y:z is 1:1:0.1, x:y:z is 1:10:0.1, x:y:z is 1:1:5, x:y:z is 1:5:1 or any other suitable ratio within the aforementioned range.

[0032] In some embodiments, R 1 Derived from one of the following compounds: divinylbenzene (DVB), butadiene; R 2Derived from one of the following compounds: styrene, 4-vinylbiphenyl, 2-vinylnaphthalene; R 3 Derived from one of the following compounds: acenaphthylene, cyclopentadiene, cyclobutadiene, norbornene, dicyclopentadiene (DCPD), and the above raw materials can be dissolved in a solvent with a Lewis acid catalyst and reacted for 6 to 8 hours at 0°C to 100°C, and then neutralized with an alkaline aqueous solution to form a copolymer. The detailed manufacturing process will be further described below, wherein the Lewis acid catalyst is, for example, SnCl 4 ·5H 2 O or BF 3 .Oet 3 The solvent is, for example, toluene or dimethylformamide (DMF), and the alkaline aqueous solution is, for example, sodium bicarbonate (NaHCO 3 ) aqueous solution. However, the present invention is not limited thereto. In other embodiments, the Lewis acid catalyst is, for example, a metal fluoride (such as SnF 4 、WF 6 , HfF 4 , ZrF 4 ) or complexes (such as WCl 6 、AlCl 3 、SbCl 3 , FeBr 3 、FeCl 3 、TiCl 4 、ZnCl 2 、NbCl 5 CF 3 SO 3 H、TiCl 3 -Al(C 2 H 5 ) 3 、TiCl 4 / LiAlH 4 、TiCl 4 / MAO、ZrCl 4 / MAO、TiCl 3 / MAO、VCl 4 / MAO、CrCl 3 / MAO、TiCl 4 / MgCl 2 、TiCl 4 / NdCl 3 、TiCl 4 / VCl3 、TiCl 4 / EtAlCl 2 、RuCl 2 (=CHPh)(PCy 3 ) 2 、RuCl 2 (=CHPh)(PCy 3 )(L), RuCl 2 (=CHCH=CH 2 )(PCy 3 )(L)).

[0033] It should be noted that the resin comprising the above copolymer may be a modified liquid rubber resin, and it may be, for example, a polyphenylene ether resin (such as SA9000 or OPE-2st), a crosslinking agent (such as TAIC), a maleimide resin (such as MIR-3000), a flame retardant (such as PQ60) and / or a filler (such as SiO 2 ), and the ratio of the aromatic monomer, the ratio of the alicyclic monomer, and the ratio of the styrene monomer can be a molar ratio, but the present invention is not limited thereto.

[0034] The following examples and comparative examples are listed to illustrate the effects of the present invention, but the scope of the present invention is not limited to the scope of the examples.

[0035] The copper foil substrates produced in the examples and comparative examples were evaluated according to the following methods.

[0036] Glass transition temperature (Tg): measured by dynamic mechanical analyzer (DMA).

[0037] Dielectric constant (10 GHz): Use a dielectric analyzer to test the dielectric constant at a frequency of 10 GHz.

[0038] Dielectric loss (10 GHz): Use a dielectric analyzer to test the dielectric loss at a frequency of 10 GHz.

[0039] Peel strength: According to the IPC-TM-650-2.4.8 test method, the peel strength of the metal substrate is tested.

[0040] Heat resistance: Heat the metal substrate in a pressure cooker at 120°C and 2atm for 120 minutes, then immerse it in a 288°C soldering furnace, and record the time required for the board to burst. If the board burst time exceeds 10 minutes (min), it is indicated as "OK", and if the board burst time is shorter than 10 minutes, it is indicated as "NG".

[0041] <Copolymer 1 to Copolymer 6>

[0042] Use the R shown in Table 1 1 , R 2 , R 3 The raw materials (alkenyl compounds, aromatic compounds and alicyclic compounds, corresponding to the chemical structure formula above) are dissolved in 24 ml of the solvent shown in Table 1 together with 0.2 g of the Lewis acid catalyst shown in Table 1 to form a first solution, and the relevant reaction conditions are also shown in Table 1, wherein the first solution can be a round-bottomed reaction flask equipped with a stirring mixed gas, nitrogen is introduced into the reaction flask to remove air and moisture, and the first solution is uniformly mixed at 300 rpm. Then, an alkaline aqueous solution (8% sodium bicarbonate aqueous solution) is used to neutralize the first solution, wherein when the reaction temperature of the first solution is greater than or equal to 70°C, the solid in the first solution is dissolved into a clear liquid and then the reaction is continued at the same temperature for 2 hours, so that the clear solution becomes a viscous solution before the neutralization reaction. Then, after filtering and vacuum drying, copolymers 1 to 6 are obtained.

[0043] Table 1

[0044]

[0045]

[0046] <Examples 1 to 6, Comparative Examples 1 to 6>

[0047] The varnish of thermosetting resin composition was formed by mixing toluene with the components in the proportions shown in Table 2. The varnish was impregnated with Nan Ya fiberglass cloth (Nan Ya Plastics Co., Ltd., cloth type 1078) at room temperature, and then dried at 130°C (impregnation machine) for several minutes to obtain a prepreg with a resin content of 60wt%. Finally, four prepregs were stacked between two 35μm thick copper foils and heated at 25kg / cm 2 The pressure and temperature were maintained at a constant temperature of 85°C for 20 minutes, and then heated to 210°C at a heating rate of 3°C / min, and then maintained at a constant temperature for 120 minutes, and then slowly cooled to 130°C to obtain 0.5 mm thick copper foil substrates of Examples 1 to 6 and Comparative Examples 1 to 6, wherein B-1000, B-2000 (NIPPON SODA) and RI 257 (CRAY VALLEY) are unmodified commercially available liquid rubber resins.

[0048] The relevant properties of the manufactured copper foil substrate were tested, and the results are shown in Table 2. After comparing the results of Examples 1 to 6 and Comparative Examples 1 to 6 in Table 2, the following conclusions can be drawn: the copper foil substrates of Examples 1 to 6 have significantly improved glass transition temperature and peel strength compared to the copper foil substrates of Comparative Examples 1 to 6 with similar other properties (such as dielectric properties and heat resistance).

[0049] Table 2

[0050]

[0051]

[0052] In summary, the resin composition of the present invention introduces a copolymer including an aromatic monomer and an alicyclic monomer, and the proportion of the alicyclic monomer is designed accordingly so that the copolymer contains a non-polar backbone structure. Therefore, a substrate (such as a circuit board or a copper foil substrate) manufactured using the same can have good low dielectric properties while improving the glass transition temperature and peel strength.

[0053] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A resin composition, characterized in that: include: The copolymer comprises an aromatic monomer and an alicyclic monomer, wherein the molecular weight of the copolymer ranges from 2000 to 5000, and the proportion of the alicyclic monomer relative to the copolymer ranges from 1% to 30%.

2. The resin composition according to claim 1, characterized in that The copolymer includes a vinyl group, and a ratio of the vinyl group is between 10% and 40% relative to the copolymer.

3. The resin composition according to claim 1, characterized in that The aromatic monomer includes a styrene monomer, and the proportion of the styrene monomer relative to the copolymer is between 20% and 90%.

4. The resin composition according to claim 1, characterized in that The copolymer has the following general chemical structure: in The R1 is The R2 is selected from at least one of the following chemical formulas: The R3 is selected from at least one of the following chemical formulas: and The x:y:z is 1:1-10:0.1-5.

5. A method for producing a resin composition, characterized in that: include: The preparation of the copolymer comprises the following steps: Dissolving at least a Lewis acid catalyst, an aromatic compound, and an alicyclic compound in a solvent to form a first solution; as well as The first solution is neutralized by using an alkaline aqueous solution, wherein the copolymer comprises an aromatic monomer and an alicyclic monomer, the molecular weight of the copolymer ranges from 2000 to 5000, and the proportion of the alicyclic monomer relative to the copolymer ranges from 1% to 30%.

6. The method for producing a resin composition according to claim 5, wherein: The copolymer has the following general chemical structure: in R1 is derived from at least one of the following compounds: divinylbenzene, butadiene; R2 is derived from at least one of the following compounds: styrene, tetravinylbiphenyl, divinylnaphthalene; R3 is derived from at least one of the following compounds: acenaphthylene, cyclopentadiene, cyclobutadiene, norbornene, dicyclopentadiene; and The x:y:z is 1:1-10:0.1-5.

7. The method for producing a resin composition according to claim 5, wherein: The Lewis acid catalyst includes SnCl4.H2O or BF3.Oet3.

8. The method for producing a resin composition according to claim 5, wherein: The solvent includes toluene or dimethylformamide.

9. The method for producing a resin composition according to claim 5, wherein: The alkaline aqueous solution includes an aqueous sodium bicarbonate solution.

10. The method for producing a resin composition according to claim 5, wherein: The reaction temperature of the neutralization reaction is greater than or equal to 70°C.