Plastic for children's toys

By using plastic toys with ingredients such as ABS, antioxidants, compatibility agents, epoxy soybean oil, isodosorbitol plasticizers and chorionic acid, the migration of phthalate plasticizers in children's plastic toys is solved. The problem of this is to achieve non-toxic, smooth, transparent and safe toys, and prevent accidental consumption by the bitter taste of bitter melon, reducing health risks.

CN119060490APending Publication Date: 2024-12-03KAMSZE FAT IND HUI ZHOUCO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411321287.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Phthalate plasticizers commonly used in children's plastic toys may migrate during use and aging, resulting in intake of children in their bodies, pose health risks, and alternative materials are needed to reduce health risks.

Method used

Plastics that use ABS, antioxidants, compatibility agents, epoxy soybean oil, isodosorbitol plasticizer, food-grade masterbatch and bitter melon are processed through specific processes to form non-toxic, smooth, Transparent and low-absorbent plastic toys, bitter melon produces a bitter taste when children lick it to avoid missed eating.

Benefits of technology

It realizes the non-toxicity and safety of children's toys. It replaces traditional plasticizers by isodidosorbate, which improves the strength and transparency of the plastics. At the same time, it prevents children from putting the toys into their mouths through the bitter taste effect of bitter melon. Effectively avoid health risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060490A_ABST
    Figure CN119060490A_ABST
Patent Text Reader

Abstract

The invention discloses a plastic for children's toys, which comprises the following components: ABS (Acrylonitrile Butadiene Styrene), an antioxidant, a compatilizer, epoxidized soybean oil, an isodidehydrated sorbitol plasticizer, food-grade color master batch, charantin and vinyl silicone oil. Compared with the prior art, the plastic toy has the following advantages that the plastic components comprise ABS, the antioxidant, the compatilizer, the epoxidized soybean oil, the isodidehydrated sorbitol plasticizer, the food-grade color master batch, the charantin and the vinyl silicone oil, so that the formed plastic toy is non-toxic and harmless, the isodidehydrated sorbitol ester is used for replacing the traditional dioctyl phthalate, and the plastic toy is environment-friendly. The charantin is good in smoothness, good in transparency and low in water absorption, and when a child licks a formed plastic toy through the charantin, the child feels bitter, and then the child is effectively prevented from stretching the toy into the mouth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of toy plastics, in particular to plastics for children's toys. Background Art

[0002] With the rapid development of the global economy, plastic products have become important items in people's daily lives, among which plastic toys are widely used in children's games and learning. Plastic toys are made of high molecular synthetic resin (polymer) as the main component, infiltrated with various additives or auxiliaries, and have plasticity and fluidity at specific temperature and pressure, can be formed into a certain shape, and can maintain a certain shape under certain conditions. Pure substances or polymer substances are produced during the polymerization process. Whether it is natural resin or synthetic resin, it is a polymer, called a macromolecule.

[0003] However, chemical substances in plastic toys, such as phthalate plasticizers, are commonly added to children's plastic toys during the production process. These plasticizers are easily migrated from the products as the toys are used and aged, which may increase the intake of phthalates in children's bodies. These substances may cause certain health risks to the human body. Therefore, how to replace phthalate plasticizers in plastic toys becomes very important. Therefore, a plastic for children's toys is provided to solve the above problems. Summary of the invention

[0004] In order to solve the problems in the above background technology, the technical solution adopted by the present invention to solve the technical problems is: a plastic for children's toys, the plastic components of which include: ABS, antioxidant, compatibilizer, epoxidized soybean oil, isosorbide plasticizer, food-grade masterbatch, momordica charantia, and vinyl silicone oil. The plastic components are divided by weight: ABS 25-35kg, antioxidant 0.5-0.9kg, compatibilizer 0.3-0.7kg, epoxidized soybean oil 0.1-0.5kg, isosorbide plasticizer 0.8-1.1kg, food-grade masterbatch 0.2-0.9kg, momordica charantia 0.01-0.07kg, and vinyl silicone oil 0.2-0.4kg.

[0005] Plastics are made from:

[0006] Step 1: Weigh 35kg of ABS, 0.9kg of antioxidant, 0.7kg of compatibilizer, 0.5kg of epoxy soybean oil, 1.1kg of iso-dianhydrosorbitol plasticizer, 0.9kg of food-grade masterbatch, 0.07kg of momordica charantia, and 0.4kg of vinyl silicone oil, pour them into a mixing container, heat to 55-75°C, and stir at 45r / min for 25-35min to mix evenly;

[0007] Step 2: Process the mixed raw materials into shapes using an injection molding machine.

[0008] As a preferred technical solution of the present invention, the vinyl silicone oil is used to enhance the strength and hardness of the silicone rubber.

[0009] As a preferred technical solution of the present invention, the food-grade masterbatch is composed of natural dyes, carrier resins, antioxidants, and compatibilizers. The carrier resin is made of ABS material, and the ABS is composed of acrylonitrile, butadiene benzene, and ethylene.

[0010] Momordica charantia is extracted by:

[0011] Step 1: Take 100g of fresh bitter gourd, add 10ml of distilled water, 42ml of 96% ethanol, and 3.5ml of concentrated sulfuric acid, homogenize at 26-30°C for 8-12min, then add 60ml of water and 260ml of 96% ethanol, stir for 8-12min and then filter, add 2.8% NH4OH to the filtrate, gradually adjust the pH value to a solution where crystals are dissolved in ethanol: NH4OH in a ratio of 1:2;

[0012] Step 2: Chromatography at 100°C for 0.5 hours, then adding a developing agent until the mobility reaches 0.20-0.25, then eluting with a solution of ethanol: NH4OH = 1: (2-3), then filtering and vacuum drying to obtain 1g of pure colorless crystals, and reflux heating 1g of colorless crystals with NH4OH for 21 hours to obtain a fresh water solution;

[0013] Step 3: Filter and dry the aqueous solution in step 2, then dissolve the dried product in 50% ethanol, and perform paper chromatography to obtain pure crystalline momordicin.

[0014] As a preferred technical solution of the present invention, in step 2, the developing agent is composed of N-butanol and acetic acid, and N-butanol: water: acetic acid = (10-12): (4-5): (1-2).

[0015] As a preferred technical solution of the present invention, the iso-dianhydrosorbitol plasticizer is prepared in the following manner:

[0016] Step 1: first add sorbitol raw material into the reactor, heat until sorbitol is melted, and then add solid acid catalyst;

[0017] Step 2: The raw material of step 1 is reacted in the absence of solvent and under reduced pressure at a reaction temperature of 180-220° C., a stirring speed of 650-750 r / min, a reaction time of 1-7 h, cooled to room temperature, and then water is added to dissolve isosorbide, and the catalyst and isosorbide are separated.

[0018] As a preferred technical solution of the present invention, the solid acid catalyst refers to WO3 / ZrO2 or Mo03 / ZrO2 catalyst, and the catalyst dosage is 5-13wt% of the mass percentage of the raw material. A negative pressure state is maintained during the reaction, and the pressure in the reactor is 1-4500Pa.

[0019] As a preferred technical solution of the present invention, the WO3 / ZrO2 and Mo03 / ZrO2 are prepared by reflux impregnation method or co-precipitation method, and the calcination temperature is 750-800°C, and the loading amount of WO3 or Mo03 is 20-35wt%.

[0020] The invention has the following advantages: the plastic components of the invention adopt ABS, antioxidant, compatibilizer, epoxy soybean oil, iso-dianhydrosorbitol plasticizer, food-grade masterbatch, momordica charantia, and vinyl silicone oil, so that the molded plastic toys are non-toxic and harmless, and the iso-dianhydrosorbitol ester replaces the traditional phthalic acid diester, and the plastic toys have good smoothness, good transparency, and low water absorption, and the momordica charantia makes the molded plastic toys feel bitter when children lick them, so that children are effectively prevented from putting the toys into their mouths. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the toy plastic production process of the preferred embodiment of the present invention. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Many specific details are explained in the following description to facilitate a full understanding of the present invention. However, the present invention can also be implemented in other ways different from those described herein. Therefore, the scope of protection of the present invention is not limited by the specific embodiments disclosed below.

[0023] In order to more clearly understand the above-mentioned objects, features and advantages of the present invention, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0024] Please refer to Figure 1The present invention discloses a plastic for children's toys. The plastic components include: ABS, antioxidant, compatibilizer, epoxy soybean oil, isosorbide plasticizer, food-grade masterbatch, momordica charantia, and vinyl silicone oil. The plastic components are divided by weight into: ABS 25-35kg, antioxidant 0.5-0.9kg, compatibilizer 0.3-0.7kg, epoxy soybean oil 0.1-0.5kg, isosorbide plasticizer 0.8-1.1kg, food-grade masterbatch 0.2-0.9kg, momordica charantia 0.01-0.07kg, and vinyl silicone oil 0.2-0.4kg.

[0025] Plastics are made from:

[0026] Step 1: Weigh 35kg of ABS, 0.9kg of antioxidant, 0.7kg of compatibilizer, 0.5kg of epoxy soybean oil, 1.1kg of iso-dianhydrosorbitol plasticizer, 0.9kg of food-grade masterbatch, 0.07kg of momordica charantia, and 0.4kg of vinyl silicone oil, pour them into a mixing container, heat to 55-75°C, and stir at 45r / min for 25-35min to mix evenly;

[0027] Step 2: The mixed raw materials are processed and molded by an injection molding machine. In the injection molding process, injection molding is used for filling, and the molding temperature during the injection molding process is 150-350°C, the injection pressure is 20-90Mpa, the pressure of the pressure holding molding is 20-100MPa, and the time of the pressure holding molding is 10-160s.

[0028] Among them, vinyl silicone oil is used to enhance the strength and hardness of silicone rubber. Food-grade masterbatch is composed of natural dyes, carrier resins, antioxidants, and compatibilizers. The carrier resin is made of ABS material, which is composed of acrylonitrile, butadiene benzene, and ethylene. Vinyl silicone oil can then be used to improve the structural strength of the plastic after molding.

[0029] Momordica charantia is extracted by:

[0030] Step 1: Take 100g of fresh bitter gourd, add 10ml of distilled water, 42ml of 96% ethanol, and 3.5ml of concentrated sulfuric acid, homogenize at 26-30°C for 8-12min, then add 60ml of water and 260ml of 96% ethanol, stir for 8-12min and then filter, add 2.8% NH4OH to the filtrate, gradually adjust the pH value to a solution where crystals are dissolved in ethanol: NH4OH in a ratio of 1:2;

[0031] Step 2: Chromatography at 100°C for 0.5 hours, then adding a developing agent until the mobility reaches 0.20-0.25, then eluting with a solution of ethanol: NH4OH = 1: (2-3), then filtering and vacuum drying to obtain 1 g of pure colorless crystals, reflux heating 1 g of colorless crystals with NH4OH for 21 hours to obtain a fresh water solution, wherein the developing agent is composed of N-butanol and acetic acid, and N-butanol: water: acetic acid = (10-12): (4-5): (1-2);

[0032] Step 3: Filter and dry the aqueous solution in step 2, then dissolve the dried product in 50% ethanol, and perform paper chromatography to obtain pure crystalline momordicin.

[0033] Isosorbide-5-nitropropene plasticizer is made by:

[0034] Step 1: first add sorbitol raw material into the reactor, heat until sorbitol is melted, and then add solid acid catalyst;

[0035] Step 2: The raw materials of step 1 are subjected to solvent-free and reduced pressure conditions at a reaction temperature of 180-220°C, a stirring speed of 650-750r / min, a reaction time of 1-7h, cooled to room temperature, and then water is added to dissolve isosorbide, and the catalyst and isosorbide are separated. The reaction temperature of the sorbitol dehydration reaction is more preferably 130-150°C, the solid acid catalyst refers to WO3 / Zr02 or Mo03 / ZrO2 catalyst, and the amount of the catalyst is 5-13wt% of the mass percentage of the raw material. A negative pressure state is maintained during the reaction, and the pressure in the reactor is 1-4500Pa. WO3 / Zr02 and Mo03 / ZrO2 are prepared by reflux impregnation or coprecipitation, and are prepared at a calcination temperature of 750-800°C, and the loading amount of WO3 or Mo03 is 20-35wt%.

[0036] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.

[0037] Other parts of the present invention not described in detail belong to the prior art and will not be described in detail here.

[0038] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A plastic for children's toys, characterized in that: The plastic components include: ABS, antioxidant, compatibilizer, epoxidized soybean oil, isosorbide plasticizer, food-grade masterbatch, momordica charantia, and vinyl silicone oil. The plastic components are divided by weight: ABS 25-35kg, antioxidant 0.5-0.9kg, compatibilizer 0.3-0.7kg, epoxidized soybean oil 0.1-0.5kg, isosorbide plasticizer 0.8-1.1kg, food-grade masterbatch 0.2-0.9kg, momordica charantia 0.01-0.07kg, and vinyl silicone oil 0.2-0.4kg.

2. A plastic for children's toys as claimed in claim 1, characterized in that: The plastic is made in the following way: Step 1: Weigh 35kg of ABS, 0.9kg of antioxidant, 0.7kg of compatibilizer, 0.5kg of epoxy soybean oil, 1.1kg of iso-dianhydrosorbitol plasticizer, 0.9kg of food-grade masterbatch, 0.07kg of momordica charantia, and 0.4kg of vinyl silicone oil, pour them into a mixing container, heat to 55-75°C, and stir at 45r / min for 25-35min to mix evenly; Step 2: Process the mixed raw materials into shapes using an injection molding machine.

3. The plastic for children's toys according to claim 1, characterized in that: The vinyl silicone oil is used to enhance the strength and hardness of silicone rubber.

4. The plastic for children's toys according to claim 1, characterized in that: The food-grade masterbatch is composed of natural dyes, carrier resin, antioxidants, and compatibilizers. The carrier resin is made of ABS material, and the ABS is composed of acrylonitrile, butadiene benzene, and ethylene.

5. The plastic for children's toys according to claim 1, characterized in that: The momordica charantia extract is extracted by the following method: Step 1: Take 100g of fresh bitter gourd, add 10ml of distilled water, 42ml of 96% ethanol, and 3.5ml of concentrated sulfuric acid, homogenize at 26-30°C for 8-12min, then add 60ml of water and 260ml of 96% ethanol, stir for 8-12min and then filter, add 2.8% NH4OH to the filtrate, gradually adjust the pH value to a solution where crystals are dissolved in ethanol: NH4OH in a ratio of 1:2; Step 2: Chromatography at 100°C for 0.5 hours, then adding a developing agent until the mobility reaches 0.20-0.25, then eluting with a solution of ethanol: NH4OH = 1: (2-3), then filtering and vacuum drying to obtain 1g of pure colorless crystals, and reflux heating 1g of colorless crystals with NH4OH for 21 hours to obtain a fresh water solution; Step 3: Filter and dry the aqueous solution in step 2, then dissolve the dried product in 50% ethanol, and perform paper chromatography to obtain pure crystalline momordicin.

6. A plastic for children's toys as claimed in claim 5, characterized in that: In step 2, the developing agent is composed of N-butanol and acetic acid, and N-butanol: water: acetic acid = (10-12): (4-5): (1-2).

7. The plastic for children's toys according to claim 1, characterized in that: The iso-bis-anhydrosorbitol plasticizer is prepared in the following manner: Step 1: first add sorbitol raw material into the reactor, heat until sorbitol is melted, and then add solid acid catalyst; Step 2: The raw material of step 1 is reacted in the absence of solvent and under reduced pressure at a reaction temperature of 180-220° C., a stirring speed of 650-750 r / min, a reaction time of 1-7 h, cooled to room temperature, and then water is added to dissolve isosorbide, and the catalyst and isosorbide are separated.

8. The plastic for children's toys as claimed in claim 7, characterized in that: The solid acid catalyst refers to WO3 / ZrO2 or Mo03 / ZrO2 catalyst, and the catalyst dosage is 5-13wt% of the mass percentage of the raw material. A negative pressure state is maintained during the reaction, and the pressure in the reactor is 1-4500Pa.

9. The plastic for children's toys as claimed in claim 8, characterized in that: The WO3 / ZrO2 and Mo03 / ZrO2 are prepared by reflux impregnation method or co-precipitation method, and are prepared at a calcination temperature of 750-800°C, and the loading amount of WO3 or Mo03 is 20-35wt%.