Biodegradable mulching film and preparation method thereof

By using modified mica sheet powder and nano silica in biodegradable mulch, the problem of insufficient barrier performance in the prior art is solved, the insulation and moisture-blocking ability of mulch film is improved, and the mechanical strength is enhanced, so as to achieve soil effective protection and release of plant nutrients.

CN119060513AActive Publication Date: 2024-12-03HENAN TECHUANG BIOTECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411330685.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

The barrier properties of existing biodegradable plastic films are insufficient, and they cannot effectively insulate and prevent soil moisture from evaporating.

Method used

Polybutylene succinate and polyhydroxy fatty acid ester are used as biodegradable resins, modified mica tablet powder, tributyl citrate and salicylic acid are added, and the preparation method of modified mica tablet powder is used to utilize poly Ethylimine modified epoxypropyldodecyldiethylammonium chloride is inserted between the layers of mica sheet powder to increase the interlayer distance and combine nano-silica to improve the dispersion and mechanical strength of mica sheet powder.

Benefits of technology

It significantly improves the barrier properties and mechanical strength of the plastic film, achieves good insulation and moisture evaporation-resistance effects on the soil, and provides the adsorption ability of nutrients and harmful substances for plant growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005056801320000051
    Figure BDA0005056801320000051
  • Figure BDA0005056801320000071
    Figure BDA0005056801320000071
  • Figure BDA0005056801320000081
    Figure BDA0005056801320000081
Patent Text Reader

Abstract

The invention relates to the technical field of polymer environment-friendly materials, in particular to a biodegradable mulching film and a preparation method thereof. Comprising the following steps: uniformly stirring and mixing poly (butylene succinate), polyhydroxyalkanoate, modified mica sheet powder, tributyl citrate, salicylic acid and 2, 4, 6-trimethyl-2, 4, 6-triphenylcyclotrisiloxane, then adding the mixture into a screw extruder for melting and plasticizing, extruding through an annular die orifice, filling dry air from the center of the die orifice, and carrying out extrusion molding to obtain a finished product. And the extruded high-temperature melt is transversely and longitudinally stretched at the same time under the combined action of a cooling air ring mounted at a die orifice, is finally led out through a traction device at the upper part of the rack, and then is led into a winding device to be wound into a finished product. The biodegradable mulching film disclosed by the invention has excellent barrier property, and has a good heat preservation effect on soil and an effect of preventing evaporation of moisture in the soil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer environmentally friendly materials, and in particular to a biodegradable ground film and a preparation method thereof. Background Art

[0002] In the agricultural field, the application of biodegradable mulch is becoming more and more widespread. Since traditional plastic mulch is often difficult to degrade after use, causing serious soil pollution, biodegradable mulch can effectively solve this problem. Biodegradable mulch is a farmland covering film made of biodegradable materials. This mulch can gradually decompose under the action of soil microorganisms and eventually convert into harmless substances such as water, carbon dioxide and biomass. According to its degradation mechanism, biodegradable mulch is mainly divided into two categories: complete biodegradation and added biodegradation. Completely biodegradable mulch is made of completely degradable materials, such as polylactic acid or polyhydroxyalkanoate. Added biodegradable mulch is to add biodegradation agents to traditional plastics to accelerate its decomposition process. In addition, depending on the raw materials, biodegradable mulch can also be subdivided into starch-based, cellulose-based, etc. These classifications are mainly based on the raw materials used to make the mulch. At present, many countries around the world are actively promoting the use of biodegradable mulch, especially in organic agriculture and green agriculture. Farmers and agricultural enterprises are increasingly aware of the environmental advantages of biodegradable mulch and have adopted it to replace traditional mulch. At the same time, the government also encourages its use by providing subsidies, tax incentives and other policy measures. With the continuous advancement of biodegradable material technology and the reduction of costs, it is expected that biodegradable mulch will play a greater role in agricultural production in the future.

[0003] Chinese patent publication number CN107325502 discloses a water-retaining, fertilizing and biodegradable agricultural mulch film and a preparation method thereof, comprising: heating the ground low-rank coal and KOH solution to 40-90°C, filtering the filtrate while hot after the reaction, cooling, adjusting the pH value to acidic, standing until no fixed matter is precipitated, and then filtering under reduced pressure, drying the filter cake to obtain low-rank coal-based humic acid; reacting the low-rank coal-based humic acid with a hydrophilic monomer, an initiator, and a cross-linking agent to prepare a low-rank coal-based humic acid super absorbent resin; taking a biodegradable material and a low-rank coal-based humic acid super absorbent resin, mixing and granulating, and blowing a film to obtain a water-retaining, fertilizing and biodegradable agricultural mulch film.

[0004] Chinese patent publication number CN113999502 discloses a UV-resistant biodegradable mulch film and a preparation method thereof, comprising the following steps: adding a two-dimensional layered material and an ultraviolet absorber to a dichloromethane solution for mixing, ultrasonically treating with a probe, and then adding a biodegradable resin and continuing to stir; centrifugally drying the obtained product to obtain an anti-UV aging component; uniformly mixing the prepared anti-aging component, biodegradable resin and other additives, and then blow molding at 160-180°C to obtain an anti-UV aging biodegradable mulch film.

[0005] Although the ground film in the above technical solution has a biodegradable function, the barrier performance of the ground film is general and cannot provide a good thermal insulation effect on the soil and prevent the evaporation of soil moisture. Summary of the invention

[0006] In order to overcome the above problems of the prior art, the present invention provides a biodegradable ground film and a preparation method thereof. The biodegradable ground film of the present invention has excellent barrier properties, has a good heat preservation effect on the soil and prevents the evaporation of water in the soil.

[0007] In order to achieve the above-mentioned invention object, the present invention adopts the following technical solutions:

[0008] A biodegradable mulch film comprises the following components in parts by weight:

[0009] 50-60 parts of polybutylene succinate, 20-30 parts of polyhydroxyalkanoate, 10-15 parts of modified mica flake powder, 1-3 parts of tributyl citrate, 1-3 parts of salicylic acid, and 0.5-1 parts of 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane.

[0010] In the technical solution of the present invention, polybutylene succinate and polyhydroxyalkanoate are used as biodegradable resins, tributyl citrate is used as a plasticizer, salicylic acid is used as a light stabilizer, and 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane is used as an ultraviolet absorber. In order to improve the barrier properties of the ground film, the present invention dopes mica flake powder into the ground film. The mica powder has a layered structure. When it is dispersed in a plastic matrix, it will form a natural barrier, thereby improving the gas barrier properties. In addition, after the resin component in the ground film is degraded, the mica flake powder can be dispersed in the soil. The mica flake powder contains a variety of nutrients required for plant growth, such as potassium, magnesium, silicon, etc. These elements can be slowly released for absorption and utilization by plants. At the same time, the mica flake powder has the ability to absorb harmful substances in the soil, such as heavy metals and organic pollutants, which helps to reduce the negative impact of these substances on plants and the environment.

[0011] Preferably, the method for preparing the modified mica flake powder comprises the following steps:

[0012] S1, adding sodium silicate and sodium dodecylbenzene sulfonate into deionized water and stirring to dissolve to obtain a mixed solution, adding mica flake powder into the mixed solution, stirring evenly to obtain a suspension;

[0013] S2, under the condition of stirring the suspension, adding hydrochloric acid to the suspension to adjust the pH to 5, heating to 50°C, keeping the temperature for reaction for 3 hours, filtering, separating, washing and drying to obtain a composite particle intermediate;

[0014] S3, calcining the composite particle intermediate in a muffle furnace, cooling, and obtaining silica-mica flake powder composite particles;

[0015] S4, adding glycidyl dodecyl diethyl ammonium chloride into deionized water, stirring and dissolving, preparing a glycidyl dodecyl diethyl ammonium chloride solution, then adding polyethyleneimine to the glycidyl dodecyl diethyl ammonium chloride solution, heating to 80° C., keeping the temperature for reaction, and performing reduced pressure distillation and vacuum drying to obtain polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride;

[0016] S5, adding silica-mica flake powder composite particles into deionized water, stirring and dispersing them evenly to obtain a suspension; adding polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride to the suspension, heating and stirring to react, and obtaining modified mica flake powder after centrifugal separation, washing, and drying.

[0017] In the technical solution of the present invention, as mentioned above, the barrier properties of the ground film are improved by doping mica flake powder in the ground film. However, since the mica flake powder is a flaky structure and the distance between layers is small, it is very easy to agglomerate in the resin during the preparation of the ground film, which affects the improvement of the barrier properties of the ground film by the mica flake powder. Therefore, the present invention modifies the mica flake powder, uses polyethyleneimine to modify glycidyl dodecyl diethyl ammonium chloride, and prepares polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride. The ability of glycidyl dodecyl diethyl ammonium chloride to insert into the mica flake powder layers is utilized to insert polyethyleneimine into the mica flake powder layers. Since polyethyleneimine is a hyperbranched molecular structure with a large steric hindrance, it can significantly increase the distance between the mica flake powder layers, thereby improving the dispersion performance of the mica flake powder in the resin, and then improving the barrier properties of the ground film.

[0018] As mentioned above, by doping mica flake powder in the film and improving its dispersibility in the resin, the barrier properties of the ground film are improved. However, a further problem is that after the mica flake powder is doped in the resin, the mechanical strength of the ground film is reduced, and the ground film is prone to cracking during the stretching step in the ground film preparation process. Therefore, the present invention further modifies the mica flake powder, using sodium silicate as a raw material and mica flake powder as a matrix, and preparing nano-silicon dioxide on the surface of the mica flake powder particles. After the nano-silicon dioxide is combined with the surface of the mica flake powder, the roughness of the surface can be increased, and the bonding force between the mica flake powder and the resin can be increased, thereby improving the mechanical strength of the ground film and avoiding the ground film from cracking due to stretching during the preparation process.

[0019] Preferably, in step S1, the mass ratio of mica flake powder to sodium silicate is 1:2-3.7.

[0020] In order to make the surface of mica flake powder combine with sufficient nano-silicon dioxide and improve the mechanical strength of the mulch, the present invention controls the mass ratio of mica flake powder to sodium silicate to be less than 1:2. However, as the amount of sodium silicate added increases, the present invention team unexpectedly discovered that when the mass ratio of mica flake powder to sodium silicate is less than 1:3.7, the barrier properties of the mulch film drop significantly. This may be because after a large amount of nano-silicon dioxide is combined on the surface of the mica flake powder, the mica flake powder has a larger surface area, and more void structures are formed between it and the resin, which in turn causes the barrier properties of the mulch film to drop. Therefore, the present invention simultaneously controls the mass ratio of mica flake powder to sodium silicate to be greater than 1:3.7.

[0021] As mentioned above, the present invention prepares nano-silicon dioxide on the surface of mica flake powder particles to improve the bonding force between mica flake powder and resin, thereby improving the mechanical strength of the ground film.

[0022] Preferably, in step S3, the calcination temperature is 450-480°C.

[0023] Preferably, in step S4, the mass ratio of glycidyl dodecyl diethyl ammonium chloride to polyethylene imine is 1:0.3-0.8.

[0024] Preferably, in step S5, the mass ratio of the silica-mica flake powder composite particles to the polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride is 1:2-5.

[0025] Preferably, in step S5, the reaction temperature is 50-60°C.

[0026] A method for preparing a biodegradable mulch film comprises the following steps:

[0027] Polybutylene succinate, polyhydroxyalkanoate, modified mica flake powder, tributyl citrate, salicylic acid and 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane are stirred and mixed evenly, then added into a screw extruder for melting and plasticization, extruded through an annular die, and dry air is filled into the center of the die, and the air acts together with a cooling air ring installed at the die to stretch the extruded high-temperature melt transversely and longitudinally at the same time, and finally led out through a traction device on the upper part of the frame, and then introduced into a winding device to obtain a finished product.

[0028] The present invention has the following beneficial effects:

[0029] 1) By adding mica flake powder into the ground film, the mica powder has a layered structure. When it is dispersed in the plastic matrix, it will form a natural barrier, thereby improving the gas barrier property, having a good heat preservation effect on the soil and preventing the evaporation of water in the soil;

[0030] 2) Using polyethyleneimine to modify glycidyl dodecyl diethyl ammonium chloride to prepare polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride, and using the ability of glycidyl dodecyl diethyl ammonium chloride to insert between mica flake powder layers, polyethyleneimine is inserted between mica flake powder layers. Since polyethyleneimine has a hyperbranched molecular structure and has a large steric hindrance, it can significantly increase the distance between mica flake powder layers, thereby improving the dispersion performance of mica flake powder in resin, and then improving the barrier performance of the ground film;

[0031] 3) Using sodium silicate as raw material and mica flake powder as matrix, nano-silicon dioxide is prepared on the surface of mica flake powder particles. After the nano-silicon dioxide is combined with the surface of mica flake powder, its surface roughness can be increased, and the bonding force between mica flake powder and resin can be increased, thereby improving the mechanical strength of the ground film and avoiding cracking of the ground film due to stretching during the preparation process. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0033] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0034] Example 1

[0035] A biodegradable mulch film comprises the following components in parts by weight:

[0036]

[0037] The preparation method of modified mica flake powder comprises the following steps:

[0038] S1, adding 10.0g sodium silicate and 0.05g sodium dodecylbenzene sulfonate into 500mL deionized water and stirring to dissolve to obtain a mixed solution, adding mica flake powder into the mixed solution, the mass ratio of mica flake powder to sodium silicate is 1:3.5, stirring evenly to obtain a suspension;

[0039] S2, under the condition of stirring the suspension, adding 5.0% hydrochloric acid to the suspension to adjust the pH to 5, heating to 50° C., keeping the temperature for reaction for 3 hours, filtering, separating, washing and drying to obtain a composite particle intermediate;

[0040] S3, placing the composite particle intermediate in a muffle furnace and calcining at 460° C. for 5 h, cooling, and obtaining silica-mica flake powder composite particles;

[0041] S4, adding 3.0 g of glycidyl dodecyl diethyl ammonium chloride to 300 mL of deionized water, stirring and dissolving, preparing a glycidyl dodecyl diethyl ammonium chloride solution, and then adding polyethyleneimine to the glycidyl dodecyl diethyl ammonium chloride solution, the mass ratio of glycidyl dodecyl diethyl ammonium chloride to polyethyleneimine being 1:0.7, heating to 80° C., keeping the temperature for reaction for 3 h, and performing reduced pressure distillation and vacuum drying to obtain polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride;

[0042] S5, add 2.0g of silica-mica flake powder composite particles into 300mL of deionized water, stir and disperse evenly to obtain a suspension; add polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride to the suspension, the mass ratio of silica-mica flake powder composite particles to polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride is 1:4, heat to 55°C, stir and react for 5h, and obtain modified mica flake powder after centrifugal separation, washing and drying.

[0043] The method for preparing a biodegradable mulch film comprises the following steps:

[0044] Polybutylene succinate, polyhydroxyalkanoate, modified mica flake powder, tributyl citrate, salicylic acid and 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane are stirred and mixed evenly, then added into a screw extruder for melting and plasticization at 200°C, extruded through an annular die, and dry air is introduced from the center of the die. The air acts together with a cooling air ring installed at the die to stretch the high-temperature melt transversely and longitudinally at the same time, transversely by 2 times, and longitudinally by 1.5 times, and finally led out through a traction device on the upper part of the frame, and then introduced into a winding device to obtain a finished product.

[0045] Example 2

[0046] A biodegradable mulch film comprises the following components in parts by weight:

[0047]

[0048] The preparation method of modified mica flake powder comprises the following steps:

[0049] S1, adding 10.0g sodium silicate and 0.05g sodium dodecylbenzene sulfonate to 500mL deionized water and stirring to dissolve to obtain a mixed solution, adding mica flake powder to the mixed solution, the mass ratio of mica flake powder to sodium silicate is 1:2.5, stirring evenly to obtain a suspension;

[0050] S2, under the condition of stirring the suspension, adding 5.0% hydrochloric acid to the suspension to adjust the pH to 5, heating to 50° C., keeping the temperature for reaction for 3 hours, filtering, separating, washing and drying to obtain a composite particle intermediate;

[0051] S3, placing the composite particle intermediate in a muffle furnace and calcining at 460° C. for 5 h, cooling, and obtaining silica-mica flake powder composite particles;

[0052] S4, adding 3.0 g of glycidyl dodecyl diethyl ammonium chloride to 300 mL of deionized water, stirring and dissolving, preparing a glycidyl dodecyl diethyl ammonium chloride solution, and then adding polyethyleneimine to the glycidyl dodecyl diethyl ammonium chloride solution, the mass ratio of glycidyl dodecyl diethyl ammonium chloride to polyethyleneimine being 1:0.4, heating to 80° C., keeping the temperature for reaction for 3 h, and performing reduced pressure distillation and vacuum drying to obtain polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride;

[0053] S5, add 2.0g of silica-mica flake powder composite particles into 300mL of deionized water, stir and disperse evenly to obtain a suspension; add polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride to the suspension, the mass ratio of silica-mica flake powder composite particles to polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride is 1:3, heat to 55°C, stir and react for 5h, and obtain modified mica flake powder after centrifugal separation, washing and drying.

[0054] The method for preparing a biodegradable mulch film comprises the following steps:

[0055] Polybutylene succinate, polyhydroxyalkanoate, modified mica flake powder, tributyl citrate, salicylic acid and 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane are stirred and mixed evenly, then added into a screw extruder for melting and plasticization at 200°C, extruded through an annular die, and dry air is introduced from the center of the die. The air acts together with a cooling air ring installed at the die to stretch the high-temperature melt transversely and longitudinally at the same time, transversely by 2 times, and longitudinally by 1.5 times, and finally led out through a traction device on the upper part of the frame, and then introduced into a winding device to obtain a finished product.

[0056] Example 3

[0057] A biodegradable mulch film comprises the following components in parts by weight:

[0058]

[0059] The preparation method of modified mica flake powder comprises the following steps:

[0060] S1, adding 10.0g sodium silicate and 0.05g sodium dodecylbenzene sulfonate into 500mL deionized water and stirring to dissolve to obtain a mixed solution, adding mica flake powder into the mixed solution, the mass ratio of mica flake powder to sodium silicate is 1:3, stirring evenly to obtain a suspension;

[0061] S2, under the condition of stirring the suspension, adding 5.0% hydrochloric acid to the suspension to adjust the pH to 5, heating to 50° C., keeping the temperature for reaction for 3 hours, filtering, separating, washing and drying to obtain a composite particle intermediate;

[0062] S3, placing the composite particle intermediate in a muffle furnace and calcining at 460° C. for 5 h, cooling, and obtaining silica-mica flake powder composite particles;

[0063] S4, adding 3.0 g of glycidyl dodecyl diethyl ammonium chloride to 300 mL of deionized water, stirring and dissolving, preparing a glycidyl dodecyl diethyl ammonium chloride solution, and then adding polyethyleneimine to the glycidyl dodecyl diethyl ammonium chloride solution, the mass ratio of glycidyl dodecyl diethyl ammonium chloride to polyethyleneimine being 1:0.6, heating to 80° C., keeping the temperature for reaction for 3 h, and performing reduced pressure distillation and vacuum drying to obtain polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride;

[0064] S5, add 2.0g of silica-mica flake powder composite particles into 300mL of deionized water, stir and disperse evenly to obtain a suspension; add polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride to the suspension, the mass ratio of silica-mica flake powder composite particles to polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride is 1:3, heat to 55°C, stir and react for 5h, and obtain modified mica flake powder after centrifugal separation, washing and drying.

[0065] The method for preparing a biodegradable mulch film comprises the following steps:

[0066] Polybutylene succinate, polyhydroxyalkanoate, modified mica flake powder, tributyl citrate, salicylic acid and 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane are stirred and mixed evenly, then added into a screw extruder for melting and plasticization at 200°C, extruded through an annular die, and dry air is introduced from the center of the die. The air acts together with a cooling air ring installed at the die to stretch the high-temperature melt transversely and longitudinally at the same time, transversely by 2 times, and longitudinally by 1.5 times, and finally led out through a traction device on the upper part of the frame, and then introduced into a winding device to obtain a finished product.

[0067] Example 4

[0068] A biodegradable mulch film comprises the following components in parts by weight:

[0069]

[0070] The preparation method of modified mica flake powder comprises the following steps:

[0071] S1, adding 10.0g sodium silicate and 0.05g sodium dodecylbenzene sulfonate into 500mL deionized water and stirring to dissolve to obtain a mixed solution, adding mica flake powder into the mixed solution, the mass ratio of mica flake powder to sodium silicate is 1:3.7, stirring evenly to obtain a suspension;

[0072] S2, under the condition of stirring the suspension, adding 5.0% hydrochloric acid to the suspension to adjust the pH to 5, heating to 50° C., keeping the temperature for reaction for 3 hours, filtering, separating, washing and drying to obtain a composite particle intermediate;

[0073] S3, calcining the composite particle intermediate in a muffle furnace at 480° C. for 5 h, and cooling to obtain silica-mica flake powder composite particles;

[0074] S4, adding 3.0 g of glycidyl dodecyl diethyl ammonium chloride to 300 mL of deionized water, stirring and dissolving, preparing a glycidyl dodecyl diethyl ammonium chloride solution, and then adding polyethyleneimine to the glycidyl dodecyl diethyl ammonium chloride solution, the mass ratio of glycidyl dodecyl diethyl ammonium chloride to polyethyleneimine being 1:0.8, heating to 80° C., keeping the temperature for reaction for 3 h, and performing reduced pressure distillation and vacuum drying to obtain polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride;

[0075] S5, add 2.0g of silica-mica flake powder composite particles into 300mL of deionized water, stir and disperse evenly to obtain a suspension; add polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride to the suspension, the mass ratio of silica-mica flake powder composite particles to polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride is 1:5, heat to 60°C, stir and react for 5h, and obtain modified mica flake powder after centrifugal separation, washing and drying.

[0076] The method for preparing a biodegradable mulch film comprises the following steps:

[0077] Polybutylene succinate, polyhydroxyalkanoate, modified mica flake powder, tributyl citrate, salicylic acid and 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane are stirred and mixed evenly, then added into a screw extruder for melting and plasticization at 200°C, extruded through an annular die, and dry air is introduced from the center of the die. The air acts together with a cooling air ring installed at the die to stretch the high-temperature melt transversely and longitudinally at the same time, transversely by 2 times, and longitudinally by 1.5 times, and finally led out through a traction device on the upper part of the frame, and then introduced into a winding device to obtain a finished product.

[0078] Example 5

[0079] A biodegradable mulch film comprises the following components in parts by weight:

[0080]

[0081]

[0082] The preparation method of modified mica flake powder comprises the following steps:

[0083] S1, adding 10.0g sodium silicate and 0.05g sodium dodecylbenzene sulfonate into 500mL deionized water and stirring to dissolve to obtain a mixed solution, adding mica flake powder into the mixed solution, the mass ratio of mica flake powder to sodium silicate is 1:2, stirring evenly to obtain a suspension;

[0084] S2, under the condition of stirring the suspension, adding 5.0% hydrochloric acid to the suspension to adjust the pH to 5, heating to 50° C., keeping the temperature for reaction for 3 hours, filtering, separating, washing and drying to obtain a composite particle intermediate;

[0085] S3, placing the composite particle intermediate in a muffle furnace and calcining at 450° C. for 5 h, cooling, and obtaining silica-mica flake powder composite particles;

[0086] S4, adding 3.0 g of glycidyl dodecyl diethyl ammonium chloride to 300 mL of deionized water, stirring and dissolving, preparing a glycidyl dodecyl diethyl ammonium chloride solution, and then adding polyethyleneimine to the glycidyl dodecyl diethyl ammonium chloride solution, the mass ratio of glycidyl dodecyl diethyl ammonium chloride to polyethyleneimine being 1:0.3, heating to 80° C., keeping the temperature for reaction for 3 h, and performing reduced pressure distillation and vacuum drying to obtain polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride;

[0087] S5, add 2.0g of silica-mica flake powder composite particles into 300mL of deionized water, stir and disperse evenly to obtain a suspension; add polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride to the suspension, the mass ratio of silica-mica flake powder composite particles to polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride is 1:2, heat to 50°C, stir and react for 5h, and obtain modified mica flake powder after centrifugal separation, washing and drying.

[0088] The method for preparing a biodegradable mulch film comprises the following steps:

[0089] Polybutylene succinate, polyhydroxyalkanoate, modified mica flake powder, tributyl citrate, salicylic acid and 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane are stirred and mixed evenly, then added into a screw extruder for melting and plasticization at 200°C, extruded through an annular die, and dry air is introduced from the center of the die. The air acts together with a cooling air ring installed at the die to stretch the high-temperature melt transversely and longitudinally at the same time, transversely by 2 times, and longitudinally by 1.5 times, and finally led out through a traction device on the upper part of the frame, and then introduced into a winding device to obtain a finished product.

[0090] Comparative Example 1

[0091] The difference between Comparative Example 1 and Example 1 is:

[0092] The mulch film composition does not contain modified mica flake powder;

[0093] The remaining steps are the same as those in Example 1.

[0094] Comparative Example 2

[0095] The difference between Comparative Example 2 and Example 1 is:

[0096] The modified mica flake powder in the mulch film component is replaced with ordinary mica flake powder.

[0097] The remaining steps are the same as those in Example 1.

[0098] Comparative Example 3

[0099] The difference between Comparative Example 3 and Example 1 is that:

[0100] The steps S1, S2 and S3 in the preparation method of modified mica powder are omitted.

[0101] That is, the surface of mica flake powder does not bind nano-silicon dioxide.

[0102] The remaining steps are the same as those in Example 1.

[0103] Comparative Example 4

[0104] The difference between Comparative Example 4 and Example 4 is that:

[0105] The mass ratio of mica flake powder to sodium silicate is 1:3.8.

[0106] The remaining steps are the same as those in Example 1.

[0107] Performance Testing

[0108] 1. Ground film barrier performance test:

[0109] The barrier properties of the mulch are characterized by the water vapor permeability. The water vapor permeability of the mulch is tested in 24 hours according to the test standard GB / T1037-2021 "Plastic Film and Sheet Water Vapor Permeability Determination Cup Weight Gain and Weight Loss Method". The test temperature is controlled at 38°C and the relative humidity is controlled at 90%.

[0110]

[0111] 2. Test of mechanical properties of ground film

[0112] 2.1. Observe with naked eyes whether there are fine cracks on the surface of the ground film to determine whether the film is damaged during the preparation process;

[0113] 2.2. Use the Q800 dynamic mechanical analyzer to test the mechanical strength of the ground film. Cut the ground film into strips of 30x10mm in size and put them into the tensile fixture, with one end fixed and the other end movable with the fixture. The preload force is 0.01N to prevent the ground film from bending during the test. The temperature is maintained at 20℃, the frequency is set to 1Hz, and the applied stress is gradually increased from 0 at a speed of 5MPa / s, and the strain change of the ground film is recorded until the ground film breaks.

[0114] The stress at the breaking point was taken as the tensile strength of the ground film. The test was repeated three times and the results were averaged.

[0115]

[0116] 3. Thermal stability test:

[0117] A temperature scanning test was performed using a Q10 differential scanning calorimeter to determine the glass transition temperature and melting temperature of the mulch film. After the mulch film was crushed, 3.5 mg was taken and placed in an aluminum crucible, which was sealed and compacted. An empty crucible was used as a blank control. The sample crucible and the empty crucible were placed in the instrument and the temperature was heated from 20°C to 300°C at a rate of 10°C / min. The average temperature of the step-down area in the thermal spectrum was taken as the glass transition temperature, and the valley temperature was taken as the melting temperature. The tests were repeated three times, and the results were averaged and expressed in the form of mean ± standard deviation. The significance was analyzed by the Duncan method.

[0118]

[0119]

[0120] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A biodegradable mulch film, characterized in that: It comprises the following components by weight: 50-60 parts of polybutylene succinate, 20-30 parts of polyhydroxyalkanoate, 10-15 parts of modified mica flake powder, 1-3 parts of tributyl citrate, 1-3 parts of salicylic acid, 2,4,6-Trimethyl-2,4,6-triphenylcyclotrisiloxane 0.5-1 part.

2. A biodegradable mulch film according to claim 1, characterized in that: Said The preparation method of modified mica flake powder comprises the following steps: S1, adding sodium silicate and sodium dodecylbenzene sulfonate into deionized water and stirring to dissolve to obtain a mixed solution, adding mica flake powder into the mixed solution, stirring evenly to obtain a suspension; S2, under the condition of stirring the suspension, adding hydrochloric acid to the suspension to adjust the pH to 5, heating to 50°C, keeping the temperature for reaction for 3 hours, filtering, separating, washing and drying to obtain a composite particle intermediate; S3, calcining the composite particle intermediate in a muffle furnace, cooling, and obtaining silica-mica flake powder composite particles; S4, adding glycidyl dodecyl diethyl ammonium chloride into deionized water, stirring and dissolving, preparing a glycidyl dodecyl diethyl ammonium chloride solution, then adding polyethyleneimine to the glycidyl dodecyl diethyl ammonium chloride solution, heating to 80° C., keeping the temperature for reaction, and performing reduced pressure distillation and vacuum drying to obtain polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride; S5, adding silica-mica flake powder composite particles into deionized water, stirring and dispersing them evenly to obtain a suspension; adding polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride to the suspension, heating and stirring to react, and obtaining modified mica flake powder after centrifugal separation, washing, and drying.

3. A biodegradable mulch film according to claim 2, characterized in that: Said In step S1, the mass ratio of mica flake powder to sodium silicate is 1:2-3.

7.

4. The biodegradable mulch film according to claim 2, characterized in that: Said In step S3, the calcination temperature is 450-480°C.

5. The biodegradable mulch film according to claim 2, characterized in that: Said In step S4, the mass ratio of glycidyl dodecyl diethyl ammonium chloride to polyethylene imine is 1:0.3-0.

8.

6. The biodegradable mulch film according to claim 2, characterized in that: Said In step S5, the mass ratio of the silica-mica flake powder composite particles to the polyethyleneimine-modified glycidyl dodecyl diethyl ammonium chloride is 1:2-5.

7. The biodegradable mulch film according to claim 2, characterized in that: Said In step S5, the reaction temperature is 50-60°C.

8. A method for preparing the biodegradable mulch film according to any one of claims 1 to 7, characterized in that: The following steps are involved: Polybutylene succinate, polyhydroxyalkanoate, modified mica flake powder, tributyl citrate, salicylic acid and 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane are stirred and mixed evenly, then added into a screw extruder for melting and plasticization, extruded through an annular die, and dry air is filled into the center of the die, and the air acts together with a cooling air ring installed at the die to stretch the extruded high-temperature melt transversely and longitudinally at the same time, and finally led out through a traction device on the upper part of the frame, and then introduced into a winding device to obtain a finished product.

Citation Information

Patent Citations

  • Biodegradable oriented composite film with high gas barrier property

    CN112250899A

  • Waterproof transparent polyimide film, preparation method and application thereof

    CN113174072A

  • Environment-friendly barrier film packing material

    CN117186597A

  • High-barrier high-mechanical-property full-biodegradable mulching film and preparation method thereof

    CN117264382A

  • Method for in-situ reinforcement of PVB (polyvinyl butyral) film material by surface modification of nano mica and product

    CN117362713A