Mechano-chemical modified halogen-free environment-friendly flame-retardant master batch as well as preparation method and application thereof

Through mechanical chemical modification technology, the dispersion of nitrogen-based and phosphorus-based flame retardant in polyamide matrix is ​​improved by using silane coupling agent and ball milling treatment, and the unstable flame retardant performance and mechanical properties in the prior art are solved. The impact problem has achieved efficient halogen-free environmentally friendly flame retardant performance and good mechanical properties.

CN119060531APending Publication Date: 2024-12-03QINGDAO UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411250633.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the nitrogen-based halogen-free flame retardant melamine cyanurate has poor dispersion in the polyamide matrix, resulting in unstable flame retardant performance, and excessive addition amount affects the mechanical properties of the material, and the phosphorus-based flame retardant compatibility It is also difficult to add evenly and affect the flame retardancy of the composite material.

Method used

Using mechanical chemical modification method, hydrogen bonds are generated by silane coupling agent and flame retardant surfactant groups and covalent bonds are formed, and the polyamide matrix is ​​combined to improve the compatibility of flame retardant and polymer, and through ball milling The treatment reduces the particle size and improves dispersion, and prepares a mechanically chemically modified halogen-free environmentally friendly flame-retardant masterbatch.

Benefits of technology

The uniform blending and good dispersion of flame retardant and polyamide matrix is ​​achieved, the flame retardant performance of UL 94V-0 standard is achieved, and the mechanical properties of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032139850000101
    Figure BDA0005032139850000101
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to a mechanochemical modified halogen-free environment-friendly flame-retardant master batch as well as a preparation method and application thereof. The flame-retardant polyamide composite material comprises the following components in parts by weight: 50-60 parts of a polyamide matrix, 40-50 parts of a flame retardant, 0.5-2 parts of a silane coupling agent and 0.2-0.5 part of an antioxidant. Through mechanochemical modification, the particle size of the flame retardant can be reduced, chemical modification of the coupling agent on the flame retardant can be promoted, and the binding force and compatibility of the flame retardant and a polyamide matrix are improved. The modification method is simple, the raw materials are cheap and easy to obtain, the prepared flame retardant is uniformly blended with a polyamide matrix, the dispersity is good, and the flame retardance reaches the UL 94V-0 standard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and specifically relates to a mechanochemically modified halogen-free environmentally friendly flame-retardant masterbatch and a preparation method and application thereof. Background Art

[0002] Polyamide is a polymer containing amide groups in the repeating units of the macromolecular chain. It is a thermoplastic engineering plastic with the largest output, the most varieties and the widest application. Polyamide has low water absorption, strong dimensional stability, excellent wear resistance, excellent flexibility and mechanical properties, and is widely used in automobiles, pipelines, 3D printing, medical and other fields. However, the flammability of polyamide is the biggest obstacle to its application, and unmodified polyamide has poor flame retardancy.

[0003] In the prior art, in order to obtain higher flame retardant properties while maintaining good mechanical properties of polyamide, additive flame retardants are usually used. Additive flame retardants mainly include halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants and inorganic flame retardants. Nitrogen / phosphorus halogen-free flame retardants are low-priced and have a wide range of raw material sources, and play an important role in flame retardant nylon. Melamine cyanurate (MCA) is a nitrogen-based halogen-free environmentally friendly flame retardant powder. Since MCA particles are rigid particles, when they are used to flame-retardantly modify nylon, they have poor dispersibility in resin, poor compatibility with the material matrix, and are prone to agglomeration, resulting in unstable flame retardant properties of the material, making it difficult to meet the UL 94V-0 standard, and excessive addition will seriously affect the mechanical properties of the material. In order to solve the problem that MCA is difficult to disperse in the resin matrix and that MCA powder is prone to dust during actual use, MCA is usually modified to further improve the flame retardant and mechanical properties of the composite material. Organophosphorus flame retardants are also difficult to add evenly to materials due to problems such as compatibility and dispersibility, which affects the flame retardancy of composite materials. Summary of the invention

[0004] The purpose of the present invention is to provide a mechanochemically modified halogen-free environmentally friendly flame retardant masterbatch and a preparation method and application thereof, so as to overcome the shortcomings of the prior art, modify the flame retardant, obtain a halogen-free environmentally friendly flame retardant masterbatch with excellent flame retardant properties, and solve the problems of uneven blending, difficult dispersion, and unstable flame retardancy of the flame retardant and the polyamide matrix in the prior art.

[0005] In order to achieve the above object, the technical solution of the present invention is:

[0006] On the one hand, the present invention provides a mechanochemically modified halogen-free environmentally friendly flame retardant masterbatch, which is composed of the following components by weight: 50 to 60 parts of a polyamide matrix, 40 to 50 parts of a flame retardant, 0.5 to 2 parts of a silane coupling agent, and 0.2 to 0.5 parts of an antioxidant.

[0007] In some other embodiments, the polyamide matrix is ​​one or more of nylon 6, nylon 66, nylon 11, nylon 612 or nylon 1012;

[0008] Preferably, the flame retardant is one or more of a nitrogen-based flame retardant or a phosphorus-based flame retardant;

[0009] Preferably, the antioxidant is one or more of antioxidant 1098, antioxidant 168 or antioxidant 9228.

[0010] In some other embodiments, the nitrogen-based flame retardant is one or more of melamine cyanurate, melamine polyphosphate or melamine hypophosphite;

[0011] The phosphorus-based flame retardant is one or more of caged pentaerythritol phosphate, phenyl phosphate, diethyl zinc hypophosphite or diethyl aluminum hypophosphite.

[0012] In some other embodiments, the silane coupling agent is γ-glycidyloxypropyltrimethoxysilane.

[0013] In a second aspect, the present invention provides a method for preparing the halogen-free, environmentally friendly, flame-retardant masterbatch according to the first aspect, comprising the following steps:

[0014] (1) mixing a silane coupling agent with a methanol aqueous solution and adding acetic acid to form a mixed solution;

[0015] (2) spraying the mixed solution in step (1) on the surface of the flame retardant, and then ball milling to obtain a modified material;

[0016] (3) separating, heat treating and cooling the material modified in step (2) to obtain a modified halogen-free environmentally friendly flame retardant;

[0017] (4) melt-blending the dried polyamide matrix and the antioxidant, and then adding the modified halogen-free environmentally friendly flame retardant obtained in step (3) for secondary melt-blending, and obtaining a mechanochemically modified halogen-free environmentally friendly flame retardant masterbatch after cooling and pelletizing.

[0018] In some other embodiments, in step (1), the volume ratio of methanol to deionized water in the methanol aqueous solution is (5-9):1;

[0019] The concentration of the silane coupling agent in the mixed solution is 10-20V%;

[0020] The pH of the mixed solution is 3-4.

[0021] In some other embodiments, in step (2), the mass ratio of the silane coupling agent to the flame retardant in the mixed solution is 1:(20-100);

[0022] The ball milling process is performed at a rotation speed of 100-200 rpm, a ball milling time of 30-60 min, and the grinding balls are zirconium dioxide balls with a particle size of 5-10 mm;

[0023] Preferably, the grinding balls are composed of Φ10 mm zirconium dioxide balls with a number percentage of 5-10%, Φ8 mm zirconium dioxide balls with a number percentage of 10-15%, and Φ5 mm zirconium dioxide balls with a number percentage of 70-80%.

[0024] In some other embodiments, in step (3), the heat treatment temperature is 100-120° C. and the drying time is 2-4 hours; in step (4), the drying of the polyamide matrix is ​​vacuum drying at 100-120° C. and the time is 2-5 hours.

[0025] In some other embodiments, in step (4),

[0026] The primary melt blending is to add the polyamide matrix and the antioxidant into the main feeding port of the screw extruder;

[0027] The secondary melt blending is to add the modified halogen-free environmentally friendly flame retardant into the side feed port of the screw extruder;

[0028] The conditions of the primary melt blending or the secondary melt blending are 230-280° C. and a rotation speed of 200-400 rpm.

[0029] In a third aspect, the present invention provides a use of the halogen-free, environmentally friendly flame-retardant masterbatch described in the first aspect in the preparation of an environmentally friendly polyamide material with flame retardancy.

[0030] Beneficial effects of the present invention:

[0031] Compared with the prior art, the present invention has the following advantages:

[0032] (1) The present invention forms hydrogen bonds between the silane coupling agent and the active groups on the surface of the flame retardant. During the heating and curing process, the silane coupling agent forms covalent bonds with the hydroxyl groups of the flame retardant accompanied by a dehydration reaction, thereby successfully modifying the flame retardant. At the same time, the organic functional groups of the silane coupling agent are combined with the polyamide matrix, thereby increasing the compatibility of the flame retardant with the polymer.

[0033] (2) The present invention reduces the particle size of the flame retardant through ball milling modification, enhances the binding property with the coupling agent, improves the dispersibility, and reduces the agglomeration phenomenon, which helps to improve the compatibility of the flame retardant with the polyamide matrix.

[0034] (3) The preparation method of the present invention is simple, the raw materials are cheap and easily available, and it is suitable for large-scale promotion and application; the flame retardant and the polyamide matrix in the prepared halogen-free environmentally friendly flame retardant masterbatch are uniformly blended, have good dispersibility, and the flame retardancy reaches the UL 94V-0 standard. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0036] The raw materials and reagents used in the following examples are all conventional commercially available products and can be purchased.

[0037] Example 1

[0038] A mechanical and chemically modified halogen-free environmentally friendly flame retardant masterbatch, which is composed of the following components by weight: melamine cyanurate (MCA): 25g, silane coupling agent KH560: 0.25ml, nylon 11: 25g, antioxidant 1098: 0.05g, antioxidant 168: 0.1g.

[0039] The preparation method adopted comprises the following steps:

[0040] (1) Weigh 25 g of nylon 11 and dry it in a vacuum drying oven at 100 °C for 2 h for later use;

[0041] (2) Weigh 9 ml of methanol solvent and 1 ml of deionized water, and add 0.1 ml of borneol acetic acid to adjust the pH value to 4 to obtain a methanol aqueous solution;

[0042] (3) Weigh 0.25 ml of coupling agent KH560 and mix it with 1 ml of methanol aqueous solution in step (2) to obtain a mixed solution with a coupling agent content of 20% by volume;

[0043] (4) Weigh 25 g of MCA flame retardant and pour it into a ball mill filled with grinding balls, take 1.25 ml of the mixed solution in step (3) and spray it evenly on the flame retardant in the ball mill (the ratio of coupling agent KH560 to MCA flame retardant is 1:100); then, ball milling is performed at a speed of 100 rpm for 30 minutes to obtain a modified material; wherein the ball milling balls used are composed of 8% Φ10 mm zirconium dioxide balls, 15% Φ8 mm zirconium dioxide balls by number, and 77% Φ5 mm zirconium dioxide balls by number;

[0044] (5) separating the modified material from the grinding balls in step (4), taking out the reaction material and placing it in an oven at 120° C. and drying it for 2 h, thereby obtaining a modified halogen-free environmentally friendly flame retardant MCA;

[0045] (6) The dried nylon 11 in step (1) is mixed with antioxidant 1098 and antioxidant 168 and added to the main feed port of the screw extruder for primary melt blending, and then the modified halogen-free environmentally friendly flame retardant MCA in step (5) is added to the side feed port of the screw extruder for secondary melt blending, and pelletized to obtain the modified halogen-free environmentally friendly flame retardant masterbatch, wherein the primary melt blending and the secondary melt blending are both at 230° C. and a rotation speed of 200 r / min.

[0046] Example 2

[0047] A mechanical and chemically modified halogen-free environmentally friendly flame retardant masterbatch, which is composed of the following components by weight: ADP / MCA composite halogen-free flame retardant in a mass ratio of 2:1: 25g, silane coupling agent KH560: 0.25ml, nylon 11: 25g, antioxidant 1098: 0.05g, antioxidant 168: 0.1g.

[0048] The preparation method used is as follows:

[0049] (1) Weigh 25 g of nylon 11 and dry it in a vacuum drying oven at 100 °C for 2 h for later use;

[0050] (2) Weigh 9 ml of methanol solvent and 1 ml of deionized water, and add 0.1 ml of borneol acetic acid to adjust the pH value to 4 to obtain a methanol aqueous solution;

[0051] (3) Weigh 0.25 ml of coupling agent KH560 and mix it with 1 ml of methanol aqueous solution in step (2) to obtain a mixed solution with a coupling agent content of 20% by volume.

[0052] (4) Weigh 25 g of ADP / MCA composite halogen-free flame retardant and pour it into a ball mill filled with grinding balls, take 1.25 ml of the mixed solution in step (3) and spray it evenly on the flame retardant in the ball mill (the feed ratio of coupling agent KH560 to MCA flame retardant is 1:100); then, ball milling is performed at a speed of 100 rpm for 40 minutes to obtain a modified material; wherein the ball milling balls used are composed of 10% Φ10 mm zirconium dioxide balls, 10% Φ8 mm zirconium dioxide balls by number, and 80% Φ5 mm zirconium dioxide balls by number;

[0053] (5) separating the modified material from the grinding balls in step (4), taking out the reaction material and placing it in an oven at 120° C. for heat treatment for 2 h, thereby obtaining a modified ADP / MCA composite halogen-free flame retardant;

[0054] (6) The dried nylon 11 in step (1) is mixed with antioxidant 1098 and antioxidant 168 and added to the main feed port of the screw extruder, and melt blended once at 230° C. and a speed of 200 r / min. Then, the modified ADPMCA composite halogen-free flame retardant in step (5) is added to the side feed port of the screw extruder, and melt blended twice. The modified halogen-free environmentally friendly flame retardant masterbatch is obtained by pelletizing, wherein the primary melt blending and the secondary melt blending are both at 250° C. and a speed of 200 r / min.

[0055] Example 3

[0056] A mechanical and chemically modified halogen-free environmentally friendly flame retardant masterbatch, which is composed of the following components by weight: melamine polyphosphate flame retardant (MPP): 7.5g, diethyl aluminum phosphite (ADP) flame retardant: 17.5g, silane coupling agent KH560: 0.25ml, nylon 11: 25g, antioxidant 1098: 0.05g, antioxidant 168: 0.1g.

[0057] The preparation method used is as follows:

[0058] (1) Weigh 25 g of nylon 11 and dry it in a vacuum drying oven at 100 °C for 2 h for later use;

[0059] (2) Weigh 9 ml of methanol solvent and 1 ml of deionized water, and add 0.1 ml of borneol acetic acid to adjust the pH value to 4 to obtain a methanol aqueous solution;

[0060] (3) Weighing 0.25 ml of coupling agent KH560 and mixing it with 1 ml of methanol aqueous solution in step (2) to obtain a mixed solution with a coupling agent content of 20% by volume;

[0061] (4) Weigh 25 g of ADP / MPP composite halogen-free flame retardant and pour it into a ball mill filled with grinding balls, take 1.25 ml of the mixed solution in step (3) and spray it evenly on the flame retardant in the ball mill (the feed ratio of coupling agent KH560 to MCA flame retardant is 1:100); then, ball milling is performed at a speed of 100 rpm for 40 minutes to obtain a modified material; wherein the ball milling balls used are composed of 10% Φ10 mm zirconium dioxide balls, 15% Φ8 mm zirconium dioxide balls by number, and 75% Φ5 mm zirconium dioxide balls by number;

[0062] (5) separating the modified material from the grinding balls in step (4), taking out the reaction material and placing it in an oven at 120° C. and drying it for 2 h, thereby obtaining a modified ADP / MPP composite halogen-free flame retardant;

[0063] (6) The dried nylon 11 in step (1) is mixed with antioxidant 1098 and antioxidant 168 and added to the main feed port of the screw extruder, and melt blended once at 230° C. and a speed of 200 r / min. Then, the modified ADP / MPP composite halogen-free flame retardant in step (5) is added to the side feed port of the screw extruder, and melt blended twice. The modified halogen-free environmentally friendly flame retardant masterbatch is obtained by pelletizing, wherein the primary melt blending and the secondary melt blending are both at 250° C. and a speed of 300 r / min.

[0064] Example 4

[0065] A mechanical and chemically modified halogen-free environmentally friendly flame retardant masterbatch, which is composed of the following components by weight: melamine cyanurate (MCA): 15g, phenyl phosphate (PFO) flame retardant: 10g, silane coupling agent KH560: 0.25ml, nylon 11: 25g, antioxidant 1098: 0.05g, antioxidant 9228: 0.1g.

[0066] The preparation method used is as follows:

[0067] (1) Weigh 25 g of nylon 11 and dry it in a vacuum drying oven at 100 °C for 2 h for later use;

[0068] (2) Weigh 9 ml of methanol solvent and 1 ml of deionized water, and add 0.1 ml of borneol acetic acid to adjust the pH value to 4 to obtain a methanol aqueous solution;

[0069] (3) Weigh 0.25 ml of coupling agent KH560 and mix it with 1 ml of methanol aqueous solution in step (2) to obtain a mixed solution with a coupling agent content of 20% by volume;

[0070] (4) Weigh 25 g of MCA / PFO composite halogen-free flame retardant and pour it into a ball mill filled with grinding balls, take 1.25 ml of the mixed solution in step (3) and spray it evenly on the flame retardant in the ball mill (the feed ratio of coupling agent KH560 to MCA flame retardant is 1:100); then, ball milling is performed at a speed of 100 rpm for 30 minutes to obtain a modified material; wherein the ball milling balls used are composed of 10% Φ10 mm zirconium dioxide balls, 15% Φ8 mm zirconium dioxide balls by number, and 75% Φ5 mm zirconium dioxide balls by number;

[0071] (5) separating the modified material from the grinding balls in step (4), taking out the reaction material and placing it in an oven at 120° C. and drying it for 2 h, thereby obtaining a modified MCA / PFO composite halogen-free flame retardant;

[0072] (6) The dried nylon 11 in step (1) is mixed with antioxidant 1098 and antioxidant 168 and added to the main feed port of the screw extruder, and melt blended once at 230° C. and a speed of 200 r / min. Then, the modified MCA / PFO composite halogen-free flame retardant in step (5) is added to the side feed port of the screw extruder, and melt blended twice. The modified halogen-free environmentally friendly flame retardant masterbatch is obtained by pelletizing, wherein the primary melt blending and the secondary melt blending are both at 250° C. and a speed of 300 r / min.

[0073] Example 5

[0074] A mechanical and chemically modified halogen-free environmentally friendly flame retardant masterbatch, which is composed of the following components by weight: masterbatch 1: MCA flame retardant: 25g, silane coupling agent KH560: 0.25ml, nylon 11: 25g, antioxidant 1098: 0.05g, antioxidant 168: 0.1g;

[0075] Masterbatch 2: PFO flame retardant: 25g, silane coupling agent KH560: 0.25ml, nylon 11: 25g, antioxidant 1098: 0.05g, antioxidant 168: 0.1g.

[0076] The preparation method of masterbatch 1 is as follows:

[0077] (1) Weigh 25 g of nylon 11 and dry it in a vacuum drying oven at 100 °C for 2 h for later use;

[0078] (2) Weigh 9 ml of methanol solvent and 1 ml of deionized water, and add 0.1 ml of borneol acetic acid to adjust the pH value to 4 to obtain a methanol aqueous solution;

[0079] (3) Weigh 0.25 ml of coupling agent KH560 and mix it with 1 ml of methanol aqueous solution in step (2) to obtain a mixed solution with a coupling agent content of 20% by volume.

[0080] (4) Weigh 25 g of MCA flame retardant and pour them into ball mills containing grinding balls, and take 1.25 ml of the mixed solution in step (3) and spray them evenly into the ball mills containing MCA (the coupling agent KH560 and MCA feed ratio is 1:100); then, ball milling is performed at a speed of 100 rpm for 40 minutes to obtain a modified material; wherein the ball milling balls used are composed of 8% Φ10 mm zirconium dioxide balls, 15% Φ8 mm zirconium dioxide balls by number, and 77% Φ5 mm zirconium dioxide balls by number;

[0081] (5) Separating the modified material from the grinding balls in step (4), taking out the reaction material and placing it in an oven at 120° C. and drying it for 2 h, thereby obtaining a modified MC flame retardant;

[0082] (6) The nylon 11 dried in step (1) is mixed with antioxidant 1098 and antioxidant 168 and added to the main feed port of the screw extruder for primary melt blending, and then the modified MCA flame retardant in step (5) is added to the side feed port of the screw extruder for secondary melt blending, and pelletized to obtain the modified halogen-free environmentally friendly flame retardant masterbatch 1, wherein the primary melt blending and the secondary melt blending are both carried out at 230° C. and a rotation speed of 200 r / min.

[0083] The preparation method of masterbatch 2 is different from that of masterbatch 1 in that the flame retardant added in step (4) is PFO flame retardant; the first melt blending and the second melt blending in step (6) are both carried out at 250° C. and 300 r / min; the other preparation steps are the same as those of masterbatch 1, and a modified halogen-free, environmentally friendly flame retardant masterbatch 2 is obtained.

[0084] Then, the modified halogen-free environmentally friendly flame retardant masterbatch 1 and the modified halogen-free environmentally friendly flame retardant masterbatch 2 are blended for use.

[0085] Comparative Example 1

[0086] Different from Example 1, the masterbatch does not contain silane coupling agent KH560, and is composed of the following components by weight: melamine cyanurate (MCA): 25 g, nylon 11: 25 g, antioxidant 1098: 0.05 g, antioxidant 168: 0.1 g.

[0087] The preparation method used is different from that of Example 1 in that step (3) is omitted; in step (4), 1.25 ml of the methanol aqueous solution in step (2) is directly sprayed on the flame retardant in the ball mill. The other preparation steps are the same as those of Example 1, and a masterbatch modified by adding no silane coupling agent KH560 is obtained.

[0088] Comparative Example 2

[0089] The composition of the masterbatch is the same as that of Example 1.

[0090] The preparation method used is different from that of Example 1 in that step (2) is omitted; in step (3), 0.25 ml of coupling agent KH560 is directly mixed with 1 ml of deionized water solution to obtain a mixed solution with a coupling agent content of 20 V%. The other preparation steps are the same as those of Example 1 to obtain a masterbatch without methanol modification.

[0091] Comparative Example 3

[0092] The composition of the masterbatch is the same as that of Example 1.

[0093] The difference between the preparation method used and that of Example 1 is that in step (2), 0.1 ml of borneol acetic acid is not added to adjust the pH value to 4. The other preparation steps are the same as those of Example 1, and a masterbatch modified by a methanol aqueous solution without pH adjustment is obtained.

[0094] Comparative Example 4

[0095] The composition of the masterbatch is the same as that of Example 1.

[0096] The difference between the preparation method used and that of Example 1 is that in step (2), 0.1 ml of borneol acetic acid is added to adjust the pH value to 1. The other preparation steps are the same as those of Example 1, and a masterbatch modified by adding a methanol aqueous solution having a pH value of 1 is obtained.

[0097] Comparative Example 5

[0098] The composition of the masterbatch is the same as that of Example 1.

[0099] The preparation method used is different from that of Example 1 in that deionized water is not added in step (2), only methanol is added, and borneol acetic acid is added to adjust the pH value to 4. The other preparation steps are the same as those of Example 1, and a masterbatch without deionized water modification is obtained.

[0100] Comparative Example 6

[0101] The composition of the masterbatch is the same as that of Example 1.

[0102] The difference between the preparation method used and that of Example 1 is that no ball milling treatment is performed in step (4), and only 1.25 ml of the mixed solution in step (3) is evenly sprayed on the MCA flame retardant. The other preparation steps are the same as those of Example 1, and a masterbatch without ball milling modification is obtained.

[0103] Comparative Example 7

[0104] Different from Embodiment 1, the masterbatch does not contain an antioxidant and is composed of the following components by weight:

[0105] Melamine cyanurate (MCA): 25g, silane coupling agent KH560: 0.25ml, nylon 11: 25g.

[0106] The preparation method used is different from that of Example 1 in that, in step (6), the nylon 11 dried in step (6) is directly added to the main feed port of the screw extruder for a melt blending, and then the modified MCA flame retardant in step (5) is added to the side feed port of the screw extruder for a second melt blending, and pelletizing is performed to obtain a modified halogen-free environmentally friendly flame retardant masterbatch. The other preparation steps are the same as those of Example 1, and a masterbatch modified without adding an antioxidant is obtained.

[0107] Comparative Example 8

[0108] The composition of the masterbatch is the same as that of Example 1.

[0109] The preparation method adopted is different from that of Example 1 in that no mechanochemical modification is performed, and the master batches are directly mixed and added to a screw extruder for melt blending, and pelletized to obtain modified halogen-free, environmentally friendly, flame-retardant master batches.

[0110] Performance Test:

[0111] The masterbatches prepared in the examples of the present invention and the comparative examples were respectively tested for vertical combustion (UL94) flame retardancy and tensile strength according to GB / T1040.2-2006 Determination of tensile properties of plastics - Part 2: Test conditions for molded and extruded plastics. The test results are shown in Table 1.

[0112] Table 1 Performance test

[0113]

[0114] It can be seen from Table 1 above that the modified halogen-free flame retardant masterbatch prepared by mechanochemistry in Examples 1-5 of the present invention has a good effect on improving the flame retardancy of PA11, solving the problems of uneven blending, difficult dispersion and unstable flame retardancy of the flame retardant and the nylon resin matrix in the prior art.

[0115] It can be seen from Comparative Examples 1-8 that the flame retardant materials not modified according to the method of the present invention have poor dispersibility of the flame retardant and compatibility with the substrate, so the flame retardant properties and mechanical properties of Comparative Examples 1-8 are worse than those of Examples 1-5.

[0116] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes that do not deviate from the spirit and principle of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A mechanochemically modified halogen-free environmentally friendly flame retardant masterbatch, characterized in that: The invention is composed of the following components by weight: 50-60 parts of polyamide matrix, 40-50 parts of flame retardant, 0.5-2 parts of silane coupling agent and 0.2-0.5 parts of antioxidant.

2. The halogen-free, environmentally friendly flame-retardant masterbatch according to claim 1, characterized in that: The polyamide matrix is ​​one or more of nylon 6, nylon 66, nylon 11, nylon 612 or nylon 1012; Preferably, the flame retardant is one or more of a nitrogen-based flame retardant or a phosphorus-based flame retardant; Preferably, the antioxidant is one or more of antioxidant 1098, antioxidant 168 or antioxidant 9228.

3. The halogen-free, environmentally friendly flame-retardant masterbatch according to claim 2, characterized in that: The nitrogen flame retardant is one or more of melamine cyanurate, melamine polyphosphate or melamine hypophosphite; The phosphorus-based flame retardant is one or more of caged pentaerythritol phosphate, phenyl phosphate, diethyl zinc hypophosphite or diethyl aluminum hypophosphite.

4. The halogen-free, environmentally friendly flame-retardant masterbatch according to claim 1, characterized in that: The silane coupling agent is γ-glycidyloxypropyltrimethoxysilane.

5. A method for preparing the halogen-free, environmentally friendly, flame-retardant masterbatch according to claim 1, characterized in that: The following steps are involved: (1) mixing a silane coupling agent with a methanol aqueous solution and adding acetic acid to form a mixed solution; (2) spraying the mixed solution in step (1) on the surface of the flame retardant, and then ball milling to obtain a modified material; (3) separating, heat treating and cooling the material modified in step (2) to obtain a modified halogen-free environmentally friendly flame retardant; (4) melt-blending the dried polyamide matrix and the antioxidant, and then adding the modified halogen-free environmentally friendly flame retardant obtained in step (3) for secondary melt-blending, and obtaining a mechanochemically modified halogen-free environmentally friendly flame retardant masterbatch after cooling and pelletizing.

6. The preparation method according to claim 5, characterized in that: In step (1), the volume ratio of methanol to deionized water in the methanol aqueous solution is (5-9):1; The concentration of the silane coupling agent in the mixed solution is 10-20V%; The pH of the mixed solution is 3-4.

7. The preparation method according to claim 5, characterized in that: In step (2), the mass ratio of the silane coupling agent to the flame retardant in the mixed solution is 1:(20-100); The ball milling process has a rotation speed of 100-200 rpm, a ball milling time of 30-60 min, and the grinding balls are zirconium dioxide balls with a particle size of 5-10 mm; Preferably, the grinding balls are composed of Φ10 mm zirconium dioxide balls with a number percentage of 5-10%, Φ8 mm zirconium dioxide balls with a number percentage of 10-15%, and Φ5 mm zirconium dioxide balls with a number percentage of 70-80%.

8. The preparation method according to claim 5, characterized in that: In step (3), the heat treatment temperature is 100-120°C for 2-4 hours; in step (4), the polyamide matrix is ​​dried in a vacuum at 100-120°C for 2-5 hours.

9. The preparation method according to claim 5, characterized in that: In step (4), The primary melt blending is to add the polyamide matrix and the antioxidant into the main feeding port of the screw extruder; The secondary melt blending is to add the modified halogen-free environmentally friendly flame retardant into the side feed port of the screw extruder; The conditions of the primary melt blending or the secondary melt blending are 230-280° C. and a rotation speed of 200-400 rpm.

10. Use of the halogen-free, environmentally friendly flame-retardant masterbatch according to any one of claims 1 to 4 in the preparation of an environmentally friendly polyamide material with flame retardancy.

Citation Information

Patent Citations

  • Continuous carbon fiber reinforced halogen-free flame retardant polyamide (PA) composite and preparation method thereof

    CN103289368A

  • Halogen-free flame-retardant polyamide master batch as well as preparation method and application thereof

    CN117165070A

  • Halogen free flame-retardant materials and method for manufacturing the same