Antibacterial polyamide and preparation method thereof
Through the combination of polyamide 56, polypentamethylene guanidine sulfate and EMA, the spontaneous aggregation and poor heat resistance of existing antibacterial agents in the medical and health field were solved, and an antibacterial polyamide was prepared to realize the antibacterial fiber. High efficiency, environmental protection and washing resistance, suitable for the preparation of antibacterial fibers or fabrics.
Patent Information
- Application Number
- CN202411028644.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing antibacterial agents have problems such as spontaneous aggregation, poor heat resistance, easy ooze, toxicity of scattered substances and impermeable washing in the medical and health field, which limits their application in polymer materials.
Using the combination of polyamide 56, polypentamide guanidine sulfate and EMA, melt-kneading is carried out through the twin screw extrusion process to prepare an antibacterial polyamide with excellent antibacterial properties and washing resistance, and through bio-based Pentyrene and anion exchange resin are treated to obtain environmentally friendly antibacterial fibers.
It achieves easy processing, washing resistance and environmentally friendly antibacterial effects, reduces corrosion to spinning machines, and shows efficient antibacterial activity and good mechanical properties in the water system.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to an antibacterial polyamide and a preparation method thereof, and belongs to the field of polyamide modification. Background Art
[0002] Antibacterial materials are a new type of materials with antibacterial and bactericidal functions, which are made by adding one or several specific antibacterial agents. The antibacterial modification of various raw materials has become a new trend in the development of the materials industry. Antibacterial products have huge market demand and bright development prospects.
[0003] Pentamethylenediamine can replace petroleum-based diamine as a key material for the synthesis of polyamide. Therefore, environmentally friendly polyamides have attracted widespread attention. Polyamide 5X has excellent properties in mechanical, wear resistance, elastic recovery, and especially hygroscopicity and dyeability, making polyamide 5X a substitute for traditional petroleum-based nylon on the market. Infectious diseases have become an extremely important issue in the global health care field. People are paying unprecedented attention to their own health, and the development of antibacterial materials has received more and more attention. Therefore, the antibacterial modification of polyamide 5X is expected to reduce the spread of diseases and is of great significance to improving people's living standards.
[0004] There are many types of antimicrobial agents, which can be roughly divided into three categories: inorganic, organic and natural according to their chemical composition. Inorganic antimicrobial agents can play a certain role in the field of medical and health care, but due to their large surface volume, they tend to spontaneously aggregate, resulting in the ineffectiveness of the antimicrobial agents or even becoming a health hazard. Natural antimicrobial agents are restricted by raw materials and processing conditions and cannot be commercialized on a large scale at present. Organic antimicrobial agents have the advantages of fast sterilization speed and wide sterilization range, but they also have problems such as poor heat resistance, easy exudation, toxicity of dissolved substances, and short service life due to poor washing resistance. Therefore, their use has great limitations. Among organic antimicrobial agents, guanidine derivatives have become promising antimicrobial agents due to their high efficiency, broad-spectrum antimicrobial activity, safety and non-toxicity. Guanidine-based polymers with good antimicrobial properties have the characteristics of good water solubility and are more convenient to use in water systems, but at the same time they also have the disadvantages of being not resistant to water washing and easy to leaching. This limits its application in polymers. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a guanidine-based antibacterial polyamide which is easy to process, washable, environmentally friendly and has excellent antibacterial properties, and is suitable for preparing antibacterial fibers or fabrics. The raw material polypentamethylene guanidine sulfate of the present invention can not only give the fiber excellent antibacterial properties, but also reduce corrosion to the spinning machine.
[0006] The first aspect of the present invention provides an antibacterial polyamide, wherein the raw materials of the antibacterial polyamide include polyamide 56, polypentamethylene guanidine sulfate and EMA, wherein the mass ratio of polyamide 56, polypentamethylene guanidine sulfate and EMA is (80-99.8):(0.1-10):(0.1-10).
[0007] The EMA of the present invention is an ethylene-methyl acrylate-glycidyl methacrylate terpolymer, wherein the mass ratio of ethylene, methyl acrylate, and glycidyl methacrylate is (65-70):(22-26):(5-10), preferably 68:24:8. The EMA can be commercially available or blended by a twin-screw extrusion process.
[0008] As one embodiment of the present invention, the mass ratio of polyamide 56, polypentamethylene guanidine sulfate and EMA is (96-99):(0.5-2.0):(0.5-2.0), and more preferably (97-98):(1-1.5):(1-1.5).
[0009] As an embodiment of the present invention, the polyamide 56 has a relative viscosity of 2.5 to 2.8, such as 2.5 or 2.73, and a melting point of 240 to 260° C., such as 253° C.
[0010] As a preferred embodiment of the present invention, the mass ratio of polypentamethylene guanidine sulfate to EMA is 1:1.
[0011] As an embodiment of the present invention, the weight fraction of the polypentamethylene guanidine sulfate in all raw materials is 0.1-10wt%, further 0.5-5.0wt%, for example 1.0wt%.
[0012] As an embodiment of the present invention, the weight fraction of EMA in all raw materials is 0.1-10wt%, further 0.5-5.0wt%, for example 1.0wt%.
[0013] As an embodiment of the present invention, the number average molecular weight of the polypentamethylene guanidine sulfate is 500-2000, further 600-1000, for example 800, 850, 900.
[0014] As a preferred embodiment of the present invention, the polypentamethylene guanidine sulfate is obtained by treating an aqueous solution of polypentamethylene guanidine hydrochloride with an anion exchange resin containing sulfate.
[0015] In some specific embodiments, the anion exchange resin is selected from a styrene-based weak base anion exchange resin or an acrylic acid-based weak base anion exchange resin.
[0016] In some embodiments, the anion exchange resin is selected from Lanxiao Any one or a combination of LX-16, LX-18, LX-60, LX-67 or LX-1180.
[0017] As an embodiment of the present invention, the polypentamethylene guanidine sulfate can be prepared by the following method: (1) after mixing bio-based pentamethylenediamine and guanidine hydrochloride, heat at 80-120°C for 0.5-3 hours to completely dissolve the guanidine acid, raise the temperature to 130-150°C for reaction for 3-8 hours, release gas, and then raise the temperature to 180-200°C for reaction for 2-4 hours to obtain a light yellow viscous liquid, cool and solidify, and vacuum dry at 80-100°C for 36-48 hours to obtain polypentamethylene guanidine hydrochloride; the molar ratio of the bio-based pentamethylenediamine to guanidine hydrochloride is (1-1.05):1; (2) preparing the polypentamethylene guanidine hydrochloride into a 0-25wt% guanidine salt aqueous solution, and then treating it with a sulfate-containing anion exchange resin, collecting the filtrate before saturation capacity, evaporating, and drying to obtain the polypentamethylene guanidine sulfate. Specifically, for example, the filtrate is evaporated to remove excess water, and vacuum dried at 80 to 100° C. for 36 to 48 hours to obtain polypentamethylene guanidine sulfate.
[0018] The bio-based pentamethylenediamine of the present invention refers to pentamethylenediamine synthesized from biomass-derived compounds such as glucose and lysine by enzyme reaction, yeast reaction or fermentation reaction in the monomer synthesis process. The bio-based content of bio-based pentamethylenediamine can be determined by a method for measuring the radioactive C14 content, such as the American Society for Testing and Materials standard ASTM-D6866 method.
[0019] The second aspect of the present invention provides a method for preparing the above antibacterial polyamide, which comprises the following steps: mixing polyamide 56, polypentamethylene guanidine sulfate and EMA, melt-kneading at 220-290° C., and cooling to obtain the antibacterial polyamide. Preferably, the mixture is mixed in a mixer and melt-kneaded using a twin-screw extruder.
[0020] In one embodiment, when a twin-screw extruder is used for melt mixing, the temperature is controlled as follows: the temperature of zone 1 is 160-240°C, the temperature of zone 2 is 190-250°C, the temperature of zone 3 is 220-280°C, the temperature of zone 4 is 230-280°C, the temperature of zone 5 is 240-280°C, and the temperature of the die head is 230-290°C. The temperature of the melt filter is 230-290°C.
[0021] In one embodiment, when a twin-screw extruder is used for melt mixing, the screw speed is 200-500 r / min, and / or the main feed speed is 30-60 r / min, and / or the aspect ratio is (35-45):1, for example 36:1.
[0022] The third aspect of the present invention further provides an antibacterial polyamide fiber, which comprises the above-mentioned antibacterial polyamide, the antibacterial polyamide fiber has an elongation at break of 20%-40%, a breaking strength of 3-5 cN / dtex, and an elastic modulus of 25-50 cN / dtex; the antibacterial rate against Escherichia coli is 65%-100%, and further 99%-99.99%.
[0023] Compared with the prior art, the implementation of the present invention has at least the following advantages:
[0024] The raw materials of polypentamethylene guanidine sulfate and bio-based polyamide 56 used in the present invention both contain bio-based pentamethylenediamine, which is green, low-carbon, more environmentally friendly, and in line with the concept of sustainable development. The combination of polypentamethylene guanidine sulfate and EMA enables the bio-based polyamide 56 fiber to obtain excellent antibacterial and mechanical properties. The raw materials of the antibacterial polyamide of the present invention are all solid, which greatly reduces the organic solvent wastewater treatment process compared to the previous experiments that need to be carried out with the participation of organic solvents, and is more environmentally friendly. The antibacterial polyamide of the present invention can be prepared by a one-step polymerization process, which has simple steps, is easy to operate, can be mass-produced, and has excellent prospects for industrial application. DETAILED DESCRIPTION
[0025] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions therein are essentially used as illustrations rather than to limit the present invention.
[0026] The following examples and comparative examples were used to obtain samples using the following detection methods:
[0027] 1) Antibacterial performance: Take 0.1g of sample, cut it into pieces, put it into 105CFU / mL Escherichia coli (E.coli ATCC 8099) bacterial solution, and shake it at 250r / min for 24h at 37℃. Take the shaken bacterial solution and dilute it to three groups of bacterial solutions of 104, 103, and 102CFU / mL in sequence. Take 0.1mL of each group of bacterial solution, inoculate it on LB nutrient agar, invert it, and culture it at 37℃ for 24h. After the cultivation is completed, count the live bacteria, and the number of bacteria observed in the blank group and the test group is recorded as A and B respectively. The antibacterial rate (R) of the sample can be calculated according to the following formula: %R=((AB) / A×100); 3 groups of parallel experiments are performed on each sample to calculate the average value to reduce the experimental error.
[0028] 2) Fiber mechanical properties test: The tensile mechanical properties of polyamide fibers were tested on a fully automatic single yarn strength tester (YG023B-Ⅲ, China) at a tensile rate of 500 mm / min. The sample clamping length was 500 mm. Each sample was tested 10 times and the average value was calculated.
[0029] In the following examples and comparative examples, polypentamethyleneguanidine sulfate was prepared in-house, and other raw materials were commercially available unless otherwise specified.
[0030] Preparation method of raw material polypentamethylene guanidine sulfate: after mixing bio-based pentamethylene diamine and guanidine hydrochloride in a molar ratio of 1:1, heat at 90°C for 1 hour, wait until the guanidine hydrochloride is completely dissolved, stir and heat to 140°C for 5 hours, release gas, continue to heat to 200°C, react for 2 hours, and after the reaction, the light yellow viscous liquid obtained is cooled and solidified, and vacuum dried at 80°C for 48 hours to obtain polypentamethylene guanidine hydrochloride with a number average molecular weight of 850. Then the obtained polypentamethylene guanidine hydrochloride is dissolved in water and passed through a Lanxiao Seplite LX-67 ion exchange resin column containing sulfate to obtain a solution of polypentamethylene guanidine sulfate, followed by rotary evaporation and drying to obtain polypentamethylene guanidine sulfate (number average molecular weight of 800), hereinafter referred to as PPGS.
[0031] Examples 1-4
[0032] Antibacterial polyamide raw materials: PA56 (melting point 255°C, relative viscosity 2.55), PPGS, EMA (the mass ratio of ethylene, methyl acrylate, and glycidyl methacrylate is 68:24:8), and the mass ratios of the three raw materials are 99:0.5:0.5 (Example 1), 98:1:1 (Example 2), 97:1.5:1.5 (Example 3), and 98:2:2 (Example 4).
[0033] The preparation method comprises the following steps: adding the above raw materials into a high-speed mixer for mixing, adding into a twin-screw extruder, controlling the temperatures of zones 1 to 5 to be 200° C., 230° C., 260° C., 270° C. and 275° C. in sequence; the screw speed is 400 r / min; the main feed speed is 40 r / min; the aspect ratio of the twin-screw extruder is 36:1; the temperature of the melt filter is 275° C.; the head temperature is 275° C.; the extruded melt enters a cooling water channel for cooling under traction, and then is pulled to a pelletizer for pelletizing to obtain antibacterial polyamide.
[0034] Embodiment 5-8
[0035] Preparation of antibacterial polyamide fiber: Dry the antibacterial polyamide prepared in Examples 1-4 to a moisture content of less than 400ppm, and then spin. Spinning steps: Melt and meter the antibacterial polyamide with a screw extruder, and spin the antibacterial polyamide pre-oriented yarn (POY) through a Titan mechanical spinning machine (36-hole spinneret); the temperatures of each area of the spinning machine are 250°C, 260°C, 285°C, 285°C, 285°C, 285°C; during spinning, control the side blowing cooling, the spinning temperature is 285°C, the spinning speed is 4200m / s, the cooling blowing speed is 0.40m / s, the stretching ratio is 1.25, the first heating roller temperature is 70°C, the second heating roller temperature is 160°C, the oil content is 1.2%, and after stretching, the antibacterial polyamide fiber is obtained. Among them, Examples 5-8 correspond to the antibacterial polyamide of Examples 1-4 respectively.
[0036] Comparative Example 1
[0037] The preparation method of the antibacterial polyamide fiber is the same as that of Example 5, except that the polyamide raw material does not contain EMA, and the mass ratio of polyamide 56 to polypentamethylene guanidine sulfate is 98:1.
[0038] Comparative Example 2
[0039] The preparation method of the antibacterial polyamide fiber is the same as that of Example 5, except that the polyamide raw material does not contain EMA, and the mass ratio of polyamide 56 to polypentamethylene guanidine sulfate is 99:0.5.
[0040] The antibacterial polyamide fiber samples prepared in the above Examples 5-8 and Comparative Examples 1-2 were tested for mechanical properties, and the results are shown in Table 1:
[0041] Table 1
[0042] serial number Example 5 Example 6 Example 7 Example 8 Comparative Example 1 Comparative Example 2 Elongation at break (%) 27.75 28.29 30.85 34.85 26.08 22.51 Breaking strength (cN / dtex) 3.93 3.86 3.62 3.34 3.91 3.83 Elastic modulus (cN / dtex) 33.69 32.86 26.56 24.44 32.28 31.05
[0043] As can be seen from Table 1, with the increase of PPGS addition, the breaking strength and elastic modulus of PA56 modified antibacterial polyamide slightly decreased. The addition of EMA is beneficial to improving the mechanical properties. For example, the difference between Example 5 and Comparative Example 1 is that the raw material of Comparative Example 1 does not contain EMA, and the mechanical properties are reduced. This may be because the epoxy group of EMA in the fiber molecular chain can react with the amine group, so that PA56, EMA and PPGS have a strong interaction, so that PPGS is evenly dispersed in the PA56 matrix, and EMA helps to form cracks and shear bands in the material, thereby improving the mechanical properties of the fiber.
[0044] The antibacterial polyamide fiber samples prepared in the above-mentioned Examples 5-8 and Comparative Examples 1-2 were knitted into socks by a knitting machine for dyeing. The socks were placed in soap water, the concentration of soap flakes for standard textile experiments was maintained at 2g / L, the ratio of soap flakes to water was 1:50, and the socks were treated at 55°C for 30min, then washed with deionized water, and dried at 50°C to obtain the pretreated socks. Acid blue 80 (Hangzhou Huaide Chemical Co., Ltd.) and neutral gray 2BL (Jiangsu Aosheng Enterprise Development Co., Ltd.) dye solutions with concentrations of 1.0wt% and 2.0wt% were prepared, and the pretreated socks were added to the dye solutions of the above composition at a mass ratio of 25:1. During the dyeing process, the temperature was raised to 98°C at a heating rate of 1°C / min and heated for 30min. After dyeing, the dyed sample was rinsed with water and then air-dried, and the antibacterial rate of the socks was tested, as shown in Table 2 below.
[0045] Table 2
[0046]
[0047] The results in Table 2 show that the dyed sock fabrics of the present application examples will have an impact on the antibacterial effect of Escherichia coli (E. coli). The antibacterial effect of the fabrics of the comparative example is significantly reduced after dyeing, and this reduction may be caused by dissolution under high temperature conditions of dyeing. The addition of EMA raw materials in the examples can alleviate this trend, indicating that the copolymer samples show enhanced washability. In addition, the antibacterial properties of the socks of Examples 6-8 of the present application can still be maintained at 99.99% after being dyed with neutral gray 2BL.
Claims
1. An antibacterial polyamide, characterized in that: The raw materials of the antibacterial polyamide include polyamide 56, polypentamethylene guanidine sulfate and EMA, wherein the mass ratio of polyamide 56, polypentamethylene guanidine sulfate and EMA is (80-99.8):(0.1-10):(0.1-10).
2. The antibacterial polyamide according to claim 1, characterized in that: The mass ratio of ethylene, methyl acrylate and glycidyl methacrylate in the EMA is (65-70):(22-26):(5-10).
3. The antibacterial polyamide according to claim 2, characterized in that: The mass ratio of ethylene, methyl acrylate and glycidyl methacrylate in the EMA is 68:24:
8.
4. The antibacterial polyamide according to claim 1, characterized in that: The relative viscosity of the polyamide 56 is 2.5-2.8, and the melting point is 240-260°C.
5. The antibacterial polyamide according to claim 1, characterized in that: The mass ratio of polyamide 56, polypentamethylene guanidine sulfate and EMA is (96-99):(0.5-2.0):(0.5-2.0), and more preferably (97-98):(1-1.5):(1-1.5).
6. The antibacterial polyamide according to claim 1, characterized in that: The number average molecular weight of the polypentamethylene guanidine sulfate is 500-2000, and further 600-1000.
7. The antibacterial polyamide according to claim 1, characterized in that: The polypentamethylene guanidine sulfate is obtained by treating an aqueous solution of polypentamethylene guanidine hydrochloride with an anion exchange resin containing sulfate groups.
8. A method for preparing the antibacterial polyamide according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: mixing polyamide 56, polypentamethylene guanidine sulfate and EMA, melting and kneading at 220-290° C., and cooling to obtain the product.
9. The preparation method according to claim 8, characterized in that: When using a twin-screw extruder for melt mixing, the temperature is controlled as follows: zone 1 temperature is 170-240°C, zone 2 temperature is 190-250°C, zone 3 temperature is 220-280°C, zone 4 temperature is 230-280°C, zone 5 temperature is 240-280°C, and die head temperature is 230-290°C.
10. An antibacterial polyamide fiber, comprising the antibacterial polyamide according to any one of claims 1 to 7, wherein the antibacterial polyamide fiber has an elongation at break of 20%-40%, a breaking strength of 3-5 cN / dtex, and an elastic modulus of 25-50 cN / dtex; and an antibacterial rate against Escherichia coli of 65%-100%, and further 99%-99.99%.