Non-intumescent fire retardant coating for steel structure, and preparation method and application thereof
By adopting a multi-layer protection system with a heterogeneous structure in non-expanded steel structure fire-retardant coatings, combined with interface agent, fire-retardant thermal insulation coatings and finishing coatings, the fire-retardant coatings in the prior art fire-retardant coatings in high-rise/super-high-rise buildings are solved. and the lack of thermal insulation achieves higher fire resistance limits and stability, meeting the fire protection needs of high-rise buildings.
Patent Information
- Application Number
- CN202411023990.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The homogeneous structure of existing non-expanded steel structure fire-retardant coatings limits its aging resistance and comprehensive performance, making it difficult to take into account both fire resistance and heat insulation, especially in high-rise/super-high-rise buildings, which is difficult to meet the long-term fire protection requirements.
Using a heterogeneous structure fire-retardant coating composed of interface agent, fire-retardant thermal insulation coating powder and finish coating, a composite layer protection system is formed through specific raw material ratios and process preparation methods, including interface layer, fire-retardant thermal insulation coating layer and finish coating The surface coating layer improves the refractory performance and stability of the coating.
It has achieved good fire resistance, aging resistance and comprehensive performance of non-expanded steel structure fireproof coatings, and can maintain volume stability in high-temperature environments, reaching the fire resistance limit of 4.0h, significantly improving the fire protection effect of high-rise/super-high-rise buildings.
Smart Images

Figure CN119060570A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, relates to fireproof materials, and in particular to a non-expansion type fireproof coating for steel structures, a preparation method and application thereof. Background Art
[0002] When a fire accident occurs in a high-rise / super high-rise building, the vertical spread speed is fast, there are many combustibles, external rescue is difficult, the risk of smoke and toxic gases is high, and the main rescue means are scarce. High-rise / super high-rise buildings still rely mainly on self-rescue. Therefore, improving the fire resistance limit of high-rise / super high-rise buildings is the primary issue to improve the fire safety of high-rise / super high-rise buildings.
[0003] Among the existing high-rise fire protection products, fireproof panels and fireproof coatings are the most mature technologies, and both can meet the fire resistance limit requirements of 3.00h-4.00h for high-rise / super-high-rise walls or load-bearing structures. However, the total cost of fireproof board fire protection measures is relatively high; in actual engineering applications, there are not many cases where the fire resistance limit of 3.00h-4.00h is achieved through fireproof panels. Compared with fireproof panels, the advantages of fireproof coatings are good deformability, which can be changed according to the shape of the steel structure, thin coatings, and under the same protection effect, the weight per unit area of fireproof coatings is less, and the load requirements for buildings are low.
[0004] Steel structure fire retardant coatings are mainly divided into intumescent steel structure fire retardant coatings and non-intumescent steel structure fire retardant coatings. In view of the high fire resistance requirements of high-rise and super-high-rise buildings, according to the performance characteristics of intumescent steel structure fire retardant coatings and non-intumescent steel structure fire retardant coatings, the two types of fire retardant coatings are suitable for different places. At present, in the domestic high-rise and super-high-rise steel structure (or fire resistance exceeds 2.50h) building fire protection design, it is recommended to use non-intumescent steel structure fire retardant coatings, which are mainly used for fire protection of load-bearing components. Intumescent fire retardant coatings are mainly used for fire protection of components with a fire resistance of less than 2.00h.
[0005] The non-expansion fire retardant coatings in the prior art all adopt homogeneous fire retardant structures of the same structure. To improve the fire resistance of the fire retardant coating, the thickness of the fire retardant layer can only be simply increased. Under high temperature conditions, the changes in the crystal form or volume of the heat insulating material, refractory material and binder of the fire retardant coating will correspondingly affect the volume stability of the fire retardant coating at high temperatures. However, the single-structure fire retardant coating of the prior art is difficult to take into account both the fire resistance and heat insulation of the fire retardant coating.
[0006] Therefore, providing a non-expanding steel structure fire retardant coating with good aging resistance and comprehensive performance, which can adapt to the characteristics of high-rise / super-high-rise fire protection and provide long-term fire protection for high-rise / super-high-rise buildings has become an urgent problem to be solved by technical personnel in this field. Summary of the invention
[0007] The purpose of the present invention is to provide a non-expanding steel structure fire retardant coating and a preparation method thereof, so as to solve the technical problem that the non-expanding fire retardant coatings in the prior art are all homogeneous and have the same structure as the homogeneous fire retardant structure, which limits the aging resistance and comprehensive performance of the fire retardant coatings.
[0008] Another object of the present invention is to provide an application of the non-expanding steel structure fire retardant coating in the preparation of a non-expanding steel structure composite protection system.
[0009] The technical solution adopted by the present invention is as follows:
[0010] The invention discloses a non-expansion steel structure fireproof coating, which comprises an interface agent, fireproof and heat-insulating coating powder and a finishing material coating.
[0011] In some embodiments of the present invention, the interface agent is made of raw materials including the following parts by weight: 90520-80 parts of flame retardant emulsion, 15-70 parts of solid mixture, 121-4 parts of alcohol ester, 11-44 parts of glass microspheres, 0.05-0.2 parts of hydroxyethyl cellulose, and 10-60 parts of water;
[0012] Preferably, the interface agent is made of raw materials including the following parts by weight: 90550-60 parts of flame retardant emulsion, 25-45 parts of solid mixture, 121-3 parts of alcohol ester, 14-30 glass microspheres, 0.08-0.12 parts of hydroxyethyl cellulose, and 10-45 parts of water.
[0013] In some embodiments of the present invention, the solid mixture is composed of silicon micropowder, silicon carbide powder, and attapulgite powder in a mass ratio of 4-16: 0.5-2: 0.05-0.2;
[0014] Preferably, the solid mixture is composed of silicon micropowder, silicon carbide powder and attapulgite powder in a mass ratio of 6-12:0.8-1.2:0.08-0.12.
[0015] In some embodiments of the present invention, the fireproof and heat-insulating coating powder is made of the following raw materials in parts by weight: 450-1800 parts of black silicate binder, 90-360 parts of white silicate binder, 75-300 parts of expanded perlite, 425-1700 parts of expanded vermiculite, 10-40 parts of floating beads, 110-440 parts of mica, 1.5-6 parts of hydroxypropyl cellulose, 0.1-0.4 parts of sodium lauryl sulfate, 2-8 parts of zirconium-containing aluminum silicate fiber, and 25-100 parts of alumina fiber;
[0016] Preferably, the fireproof and heat-insulating coating powder is made of raw materials including the following parts by weight: 600-1200 parts of black silicate binder, 150-210 parts of white silicate binder, 100-200 parts of expanded perlite, 700-1000 parts of expanded vermiculite, 15-25 parts of floating beads, 180-250 parts of mica, 2-4 parts of hydroxypropyl cellulose, 0.1-0.3 parts of sodium lauryl sulfate, 3-5 parts of zirconium-containing aluminum silicate fiber, and 40-60 parts of alumina fiber.
[0017] In some embodiments of the present invention, the finishing paint is made of the following raw materials in parts by weight: 10-40 parts of diatomaceous earth, 6-24 parts of closed-cell perlite, 40-160 parts of expanded vermiculite, 10-40 parts of microspheres, 100-400 parts of alumina fiber, 250-1000 parts of aluminum silicate fiber, 5-20 parts of titanium dioxide, 2-8 parts of zirconium-containing aluminum silicate fiber, 1.5-6 parts of polyvinyl alcohol powder, 15-60 parts of latex powder, and 0.1-0.4 parts of turquoise blue;
[0018] Preferably, the finishing paint is made of raw materials including the following parts by weight: 10-30 parts of diatomaceous earth, 8-16 parts of closed-cell perlite, 60-100 parts of expanded vermiculite, 10-30 parts of microspheres, 10-300 parts of alumina fiber, 400-600 parts of aluminum silicate fiber, 8-12 parts of titanium dioxide, 2-6 parts of zirconium-containing aluminum silicate fiber, 2-5 parts of polyvinyl alcohol powder, 20-40 parts of latex powder, and 0.15-0.3 parts of turquoise blue.
[0019] In some embodiments of the present invention, the interface agent is made of the following raw materials in parts by weight: 90540 parts of flame retardant emulsion, 35 parts of solid mixture, 122 parts of alcohol ester, 22 parts of glass microspheres, 0.1 parts of hydroxyethyl cellulose, and 20-30 parts of water; the solid mixture is composed of silicon micropowder: silicon carbide powder: attapulgite powder in a mass ratio of 8:1:0.1;
[0020] The fireproof and heat-insulating coating powder is made of the following raw materials in parts by weight: 900 parts of black silicate binder, 180 parts of white silicate binder, 150 parts of expanded perlite, 850 parts of expanded vermiculite, 20 parts of floating beads, 220 parts of mica, 3 parts of hydroxypropyl cellulose, 0.2 parts of sodium lauryl sulfate, 4 parts of zirconium-containing aluminum silicate fiber, and 50 parts of alumina fiber;
[0021] The finishing paint is made of raw materials including the following parts by weight: 20 parts of diatomaceous earth, 12 parts of closed-cell perlite, 80 parts of expanded vermiculite, 20 parts of microspheres, 200 parts of alumina fiber, 500 parts of aluminum silicate fiber, 10 parts of titanium dioxide, 4 parts of zirconium-containing aluminum silicate fiber, 3 parts of polyvinyl alcohol powder, 30 parts of latex powder, and 0.2 parts of turquoise blue.
[0022] In some embodiments of the present invention, the particle size of the closed-cell perlite is 80-120 mesh, preferably 100 mesh;
[0023] Or / and the particle size of expanded vermiculite is 180-220 mesh, preferably 200 mesh;
[0024] The particle size of the microbeads is 120-180 mesh, preferably 150 mesh.
[0025] The present invention discloses a method for preparing a non-expansive steel structure fire retardant coating, comprising the following steps:
[0026] Preparation of interface agent: prepare various raw materials of interface agent in proportion and mix them evenly;
[0027] Preparation of fireproof and heat-insulating coating: prepare various raw materials of fireproof and heat-insulating coating in proportion, mix them evenly, and obtain the coating;
[0028] Preparation of finishing material coating: prepare various raw materials of finishing material coating according to proportion, mix well and you have it.
[0029] The invention discloses an application of a non-expansion type steel structure fire retardant coating in preparing a non-expansion type steel structure multi-layer protection system.
[0030] The present invention discloses a non-expansion steel structure multilayer protection system, which is made of the above-mentioned non-expansion steel structure fire retardant coating, including an interface layer, a fireproof and heat-insulating coating layer and a finishing coating layer;
[0031] Among them, the interface layer is formed by evenly coating the interface agent on the surface of the steel structure; the fireproof and heat-insulating coating layer is formed by applying the fireproof and heat-insulating coating containing the interface agent; the finishing coating layer is formed by applying the finishing coating containing the interface agent;
[0032] Preferably, the fire retardant coating containing the interface agent is a mixture of fire retardant and heat insulating coating, water, and the interface agent in a mass ratio of 80 to 120:13 to 170:3 to 8, more preferably fire retardant and heat insulating coating: water: interface agent = 100:150:5;
[0033] Preferably, the finishing paint containing the interface agent is a mixture of finishing paint, water and interface agent in a mass ratio of 80-120:13-170:6-10, more preferably finishing paint: water: interface agent = 100:150:8.
[0034] When the non-expanding steel structure fire retardant coating of the present invention is used for a steel structure, the surface of the steel structure is cleaned and painted with anti-rust paint, and the interface agent is evenly applied to the surface of the steel structure. When the interface layer is not completely dry, the fire retardant coating containing the interface agent is sprayed once, and then the fire retardant coating containing the interface agent is applied once to a specified thickness. Finally, the finishing coating containing the interface agent is applied once to a specified thickness and maintained.
[0035] The applicant found in the study that the addition of cement and silicate binder can easily cause the interface agent to gel. Some acidic emulsions such as vinacetic acid emulsion, vinacetic acid propylene emulsion, tertiary carbonate emulsion, ethylene vinyl acetate copolymer emulsion have poor water resistance and are not suitable for outdoor non-expansion fire retardant coatings. Silicone acrylic emulsion has the best water resistance, but silicone acrylic emulsion can easily cause the interface agent to gel quickly. The addition of cement can improve the water resistance of the emulsion.
[0036] The applicant found that in the heating range of 400°C-1200°C, as the temperature increases, the overall volume trend of the white silicate binder is to decrease, while the overall volume trend of the black silicate binder is to increase. Relying on a single white silicate binder or a black silicate binder is not conducive to maintaining the volume stability of the fire retardant coating at high temperatures. Therefore, the present invention adopts a composite system of white silicate and black silicate binders.
[0037] The applicant found that as the temperature rises, the volume of basalt fiber gradually decreases, but the reduction is not obvious. When the temperature rises to around 1150°C, the volume of basalt fiber shrinks sharply. There are some risks when basalt is used as a refractory material. But it can be used as a thermal insulation material for multi-layer fire retardant coatings. During the heating process, as the temperature rises, the volume of mineral wool fiber expands, and then decreases and increases. When the temperature of mineral wool fiber exceeds about 950°C, the volume of mineral wool increases. The characteristics of mineral wool can be used, combined with the characteristics of black silicate temperature volume increase, to prepare a fireproof and heat-insulating layer with a relatively stable volume. Between 400°C and 550°C, the volume of carbon fiber changes little, which shows that carbon fiber is relatively stable in this temperature range. When the temperature exceeds about 550°C, the carbon fiber pixels shrink sharply linearly. This shows that when the temperature reaches 550°C, carbon fiber cannot be used as a reinforcing material for fire retardant coatings. During the entire heating process, the volume of zirconium-containing aluminum silicate fiber is relatively stable at high temperatures and can be used as a reinforcing material for fire retardant coatings.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The non-expansion steel structure fireproof coating of the present invention consists of three parts: an interface agent, a fireproof and heat-insulating coating and a finishing coating, has a heterogeneous structure, and has good fireproofing performance, aging resistance and comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Attached Figure 1 This is a schematic diagram of the thermocouple arrangement of Test Example 1;
[0041] Attached Figure 2 This is the appearance of the steel beam after the fire resistance test of Test Example 1. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, the conditions recommended by the conventional conditions or reagent providers are used. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0043] Example 1
[0044] This embodiment discloses a method for preparing a fire retardant coating of the present invention, which is specifically as follows:
[0045] 1. Preparation of interface agent
[0046] Table 1-1 Ingredients of Interface Agent in Example 1
[0047]
[0048] The production steps of the interface agent are as follows:
[0049] (1) Weigh the materials in Table 1-1 according to the proportions;
[0050] (2) Add water to the mixing tank in sequence and pour in 1 / 2 portion of alcohol ester 12;
[0051] (3) Start the mixer at a speed of 1500 r / min, slowly add the measured amount of hydroxyethyl cellulose, and stir for 20 min;
[0052] (4) Adjust the mixer speed to 900 r / min and slowly add the solid mixture into the mixing tank;
[0053] (5) Pour the measured amount of flame retardant emulsion 905 into the mixture while stirring;
[0054] (6) Pour the remaining alcohol ester 12;
[0055] (7) Reduce the speed of the mixer to 500 r / min and slowly add the vitrified microspheres;
[0056] (8) Continue stirring for 20 minutes to obtain a uniform and thick interface agent.
[0057] 2. Production of fireproof and heat-insulating coating powder
[0058] Table 1-2 Ingredients of fireproof and heat-insulating coating of Example 1
[0059] Serial number Raw material name Weight 1 Black silicate binder 900 2 White silicate binder 180 3 Expanded Perlite 150 4 Expanded Vermiculite 850 5 Floating beads 20 6 Mica 220 7 Hydroxypropyl Cellulose 3 8 Sodium Lauryl Sulfate 0.2 9 Zirconium-containing aluminum silicate fiber 4 10 Alumina Fiber 50
[0060] The production steps of fire retardant and heat insulation coating are as follows:
[0061] (1) Weigh the materials in Table 1-2 according to the proportion;
[0062] (2) Start the dry powder mixer, add measured amounts of zirconium-containing aluminum silicate fiber and aluminum oxide fiber in sequence, and stir for about 5 minutes to fully disperse the fibers;
[0063] (3) Add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium lauryl sulfate to the dry powder mixer in sequence, and continue stirring for 4 minutes after the feeding is completed;
[0064] (4) Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fire-retardant and heat-insulating coating.
[0065] 3. Production of finishing paint
[0066] Table 1-3 Ingredients of finishing coating in Example 1
[0067] Serial number Raw material name Weight 1 diatomite 20 2 Closed-cell perlite (80 mesh) 12 3 Expanded Vermiculite (220 mesh) 80 4 Microbeads (180 mesh) 20 5 Alumina Fiber 200 6 Aluminum silicate fiber 500 7 Titanium dioxide 10 8 Zirconium-containing aluminum silicate fiber 4 9 Polyvinyl alcohol powder 3 10 Latex powder 30 11 Turquoise 0.2
[0068] The production steps of finishing layer powder are as follows:
[0069] (1) Weigh the materials in Table 1-3 according to the proportion;
[0070] (2) Start the dry powder mixer, add the measured materials in sequence, and stir for about 30 minutes to fully disperse the fibers to obtain the finishing coating.
[0071] Example 2
[0072] This embodiment discloses a method for preparing a fire retardant coating of the present invention, which is specifically as follows:
[0073] 1. Preparation of interface agent
[0074] Table 2-1 Ingredients of Interface Agent in Example 2
[0075]
[0076] The production steps of the interface agent are as follows:
[0077] (1) Weigh the materials in Table 2-1 according to the proportions;
[0078] (2) Add water to the mixing tank in sequence and pour in 1 / 3 of the alcohol ester 12;
[0079] (3) Start the mixer at a speed of 1000 r / min, slowly add the measured amount of hydroxyethyl cellulose, and stir for 30 min;
[0080] (4) Adjust the mixer speed to 800 r / min and slowly add the solid mixture into the mixing tank;
[0081] (5) Pour the measured amount of flame retardant emulsion 905 into the mixture while stirring;
[0082] (6) Pour the remaining alcohol ester 12;
[0083] (7) Reduce the speed of the mixer to 400 r / min and slowly add the vitrified microspheres;
[0084] (8) Continue stirring for 30 minutes to obtain a uniform and thick interface agent.
[0085] 2. Production of fireproof and heat-insulating coating powder
[0086] Table 2-2 Ingredients of fireproof and heat-insulating coating of Example 2
[0087]
[0088]
[0089] The production steps of fire retardant and heat insulation coating are as follows:
[0090] (1) Weigh the materials in Table 2-2 according to the proportion;
[0091] (2) Start the dry powder mixer, add measured amounts of zirconium-containing aluminum silicate fibers and aluminum oxide fibers in sequence, and stir for about 10 minutes to fully disperse the fibers;
[0092] (3) Add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium lauryl sulfate to the dry powder mixer in sequence, and continue stirring for 10 minutes after the feeding is completed;
[0093] (4) Finally, add black silicate binder and white silicate binder and continue stirring for 20 minutes to obtain the fire-retardant and heat-insulating coating.
[0094] 3. Production of finishing paint
[0095] Table 2-3 Ingredients of finishing coating in Example 2
[0096] Serial number Raw material name Weight 1 diatomite 10 2 Closed-cell perlite (120 mesh) 6 3 Expanded Vermiculite (180 mesh) 40 4 Microbeads (120 mesh) 10 5 Alumina Fiber 120 6 Aluminum silicate fiber 250 7 Titanium dioxide 8 8 Zirconium-containing aluminum silicate fiber 2 9 Polyvinyl alcohol powder 2 10 Latex powder 15 11 Turquoise 0.1
[0097] The production steps of finishing layer powder are as follows:
[0098] (1) Weigh the materials in Table 2-3 according to the proportion;
[0099] (2) Start the dry powder mixer, add the measured materials in sequence, and stir for about 30 minutes to fully disperse the fibers to obtain the finishing coating.
[0100] Example 3
[0101] This embodiment discloses a method for preparing a fire retardant coating of the present invention, which is specifically as follows:
[0102] 1. Preparation of interface agent
[0103] Table 3-1 Ingredients of Interface Agent in Example 3
[0104]
[0105] The production steps of the interface agent are as follows:
[0106] (1) Weigh the materials in Table 3-1 according to the proportions;
[0107] (2) Add water to the mixing tank in sequence and pour in 1 / 2 portion of alcohol ester 12;
[0108] (3) Start the mixer at a speed of 1800 r / min, slowly add the measured amount of hydroxyethyl cellulose, and stir for 30 min;
[0109] (4) Adjust the mixer speed to 900 r / min and slowly add the solid mixture into the mixing tank;
[0110] (5) Pour the measured amount of flame retardant emulsion 905 into the mixture while stirring;
[0111] (6) Pour the remaining alcohol ester 12;
[0112] (7) Reduce the speed of the mixer to 600 r / min and slowly add the vitrified microspheres;
[0113] (8) Continue stirring for 30 minutes to obtain a uniform and thick interface agent.
[0114] 2. Production of fireproof and heat-insulating coating powder
[0115] Table 3-2 Ingredients of fireproof and heat-insulating coating of Example 3
[0116] Serial number Raw material name Weight 1 Black silicate binder 600 2 White silicate binder 110 3 Expanded Perlite 120 4 Expanded Vermiculite 425 5 Floating beads 15 6 Mica 110 7 Hydroxypropyl Cellulose 1.5 8 Sodium Lauryl Sulfate 0.1 9 Zirconium-containing aluminum silicate fiber 2 10 Alumina Fiber 25
[0117] The production steps of fire retardant and heat insulation coating are as follows:
[0118] (1) Weigh the materials in Table 3-2 according to the proportion;
[0119] (2) Start the dry powder mixer, add measured amounts of zirconium-containing aluminum silicate fiber and aluminum oxide fiber in sequence, and stir for about 5 minutes to fully disperse the fibers;
[0120] (3) Add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium lauryl sulfate to the dry powder mixer in sequence, and continue stirring for 5 minutes after the feeding is completed;
[0121] (4) Finally, add black silicate binder and white silicate binder and continue stirring for 15 minutes to obtain the fire-retardant and heat-insulating coating.
[0122] 3. Production of finishing paint
[0123] Table 3-3 Ingredients of finishing coating in Example 3
[0124] Serial number Raw material name Weight 1 diatomite 30 2 Closed-cell perlite (100 mesh) 16 3 Expanded Vermiculite (200 mesh) 40 4 Microbeads (180 mesh) 15 5 Alumina Fiber 280 6 Aluminum silicate fiber 600 7 Titanium dioxide 12 8 Zirconium-containing aluminum silicate fiber 6 9 Polyvinyl alcohol powder 5 10 Latex powder 35 11 Turquoise 0.15
[0125] The production steps of finishing layer powder are as follows:
[0126] (1) Weigh the materials in Table 3-3 according to the proportion;
[0127] (2) Start the dry powder mixer, add the measured materials in turn, and stir for about 20 minutes to fully disperse the fibers to obtain the finishing coating.
[0128] Example 4
[0129] This embodiment discloses a method for preparing a fire retardant coating of the present invention, which is specifically as follows:
[0130] 1. Preparation of interface agent
[0131] Table 4-1 Ingredients of Interface Agent in Example 4
[0132]
[0133] The production steps of the interface agent are as follows:
[0134] (1) Weigh the materials in Table 4-1 according to the proportions;
[0135] (2) Add water to the mixing tank in sequence and pour in 2 / 3 of the alcohol ester 12;
[0136] (3) Start the mixer at a speed of 1800 r / min, slowly add the measured amount of hydroxyethyl cellulose, and stir for 30 min;
[0137] (4) Adjust the mixer speed to 800 r / min and slowly add the solid mixture into the mixing tank;
[0138] (5) Pour the measured amount of flame retardant emulsion 905 into the mixture while stirring;
[0139] (6) Pour the remaining alcohol ester 12;
[0140] (7) Reduce the speed of the mixer to 400 r / min and slowly add the vitrified microspheres;
[0141] (8) Continue stirring for 10 minutes to obtain a uniform and thick interface agent.
[0142] 2. Production of fireproof and heat-insulating coating powder
[0143] Table 4-2 Ingredients of fireproof and heat-insulating coating of Example 4
[0144] Serial number Raw material name Weight 1 Black silicate binder 1200 2 White silicate binder 150 3 Expanded Perlite 100 4 Expanded Vermiculite 700 5 Floating beads 20 6 Mica 300 7 Hydroxypropyl Cellulose 3 8 Sodium Lauryl Sulfate 0.2 9 Zirconium-containing aluminum silicate fiber 5 10 Alumina Fiber 40
[0145] The production steps of fire retardant and heat insulation coating are as follows:
[0146] (1) Weigh the materials in Table 4-2 according to the proportion;
[0147] (2) Start the dry powder mixer, add measured amounts of zirconium-containing aluminum silicate fiber and aluminum oxide fiber in sequence, and stir for about 5 minutes to fully disperse the fibers;
[0148] (3) Add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium lauryl sulfate to the dry powder mixer in sequence, and continue stirring for 4 minutes after the feeding is completed;
[0149] (4) Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fire-retardant and heat-insulating coating.
[0150] 3. Production of finishing paint
[0151] Table 4-3 Ingredients of finishing coating in Example 4
[0152] Serial number Raw material name Weight 1 diatomite 40 2 Closed-cell perlite (120 mesh) 24 3 Expanded Vermiculite (200 mesh) 160 4 Microbeads (150 mesh) 40 5 Alumina Fiber 300 6 Aluminum silicate fiber 1000 7 Titanium dioxide 20 8 Zirconium-containing aluminum silicate fiber 8 9 Polyvinyl alcohol powder 6 10 Latex powder 60 11 Turquoise 0.4
[0153] The production steps of finishing layer powder are as follows:
[0154] (1) Weigh the materials in Table 4-3 according to the proportion;
[0155] (2) Start the dry powder mixer, add the measured materials in sequence, and stir for about 30 minutes to fully disperse the fibers to obtain the finishing coating.
[0156] Example 5
[0157] This embodiment discloses a method for preparing a fire retardant coating of the present invention, which is specifically as follows:
[0158] 1. Preparation of interface agent
[0159] Table 5-1 Ingredients of Interface Agent in Example 5
[0160]
[0161] The production steps of the interface agent are as follows:
[0162] (1) Weigh the materials in Table 5-1 according to the proportions;
[0163] (2) Add water to the mixing tank in sequence and pour in 1 / 2 portion of alcohol ester 12;
[0164] (3) Start the mixer at a speed of 1500 r / min, slowly add the measured amount of hydroxyethyl cellulose, and stir for 20 min;
[0165] (4) Adjust the mixer speed to 900 r / min and slowly add the solid mixture into the mixing tank;
[0166] (5) Pour the measured amount of flame retardant emulsion 905 into the mixture while stirring;
[0167] (6) Pour the remaining alcohol ester 12;
[0168] (7) Reduce the speed of the mixer to 500 r / min and slowly add the vitrified microspheres;
[0169] (8) Continue stirring for 20 minutes to obtain a uniform and thick interface agent.
[0170] 2. Production of fireproof and heat-insulating coating powder
[0171] Table 5-2 Ingredients of fireproof and heat-insulating coating of Example 5
[0172] Serial number Raw material name Weight 1 Black silicate binder 1500 2 White silicate binder 210 3 Expanded Perlite 300 4 Expanded Vermiculite 1000 5 Floating beads 40 6 Mica 250 7 Hydroxypropyl Cellulose 6 8 Sodium Lauryl Sulfate 0.4 9 Zirconium-containing aluminum silicate fiber 8 10 Alumina Fiber 60
[0173] The production steps of fire retardant and heat insulation coating are as follows:
[0174] (1) Weigh the materials in Table 5-2 according to the proportion;
[0175] (2) Start the dry powder mixer, add measured amounts of zirconium-containing aluminum silicate fiber and aluminum oxide fiber in sequence, and stir for about 5 minutes to fully disperse the fibers;
[0176] (3) Add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium lauryl sulfate to the dry powder mixer in sequence, and continue stirring for 4 minutes after the feeding is completed;
[0177] (4) Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fire-retardant and heat-insulating coating.
[0178] 3. Production of finishing paint
[0179] Table 5-3 Ingredients of finishing coating in Example 5
[0180]
[0181]
[0182] The production steps of finishing layer powder are as follows:
[0183] (1) Weigh the materials in Table 5-3 according to the proportion;
[0184] (2) Start the dry powder mixer, add the measured materials in sequence, and stir for about 30 minutes to fully disperse the fibers to obtain the finishing coating.
[0185] Example 6
[0186] This embodiment discloses a method for preparing a fire retardant coating of the present invention, which is specifically as follows:
[0187] 1. Preparation of interface agent
[0188] Table 6-1 Ingredients of Interface Agent in Example 6
[0189]
[0190] The production steps of the interface agent are as follows:
[0191] (1) Weigh the materials in Table 6-1 according to the proportions;
[0192] (2) Add water to the mixing tank in sequence and pour in 1 / 2 portion of alcohol ester 12;
[0193] (3) Start the mixer at a speed of 1500 r / min, slowly add the measured amount of hydroxyethyl cellulose, and stir for 20 min;
[0194] (4) Adjust the mixer speed to 900 r / min and slowly add the solid mixture into the mixing tank;
[0195] (5) Pour the measured amount of flame retardant emulsion 905 into the mixture while stirring;
[0196] (6) Pour the remaining alcohol ester 12;
[0197] (7) Reduce the speed of the mixer to 500 r / min and slowly add the vitrified microspheres;
[0198] (8) Continue stirring for 20 minutes to obtain a uniform and thick interface agent.
[0199] 2. Production of fireproof and heat-insulating coating powder
[0200] Table 6-2 Ingredients of fireproof and heat-insulating coating of Example 6
[0201]
[0202]
[0203] The production steps of fire retardant and heat insulation coating are as follows:
[0204] (1) Weigh the materials in Table 6-2 according to the proportion;
[0205] (2) Start the dry powder mixer, add measured amounts of zirconium-containing aluminum silicate fiber and aluminum oxide fiber in sequence, and stir for about 5 minutes to fully disperse the fibers;
[0206] (3) Add expanded perlite, expanded vermiculite, floating beads, mica, hydroxypropyl cellulose, and sodium lauryl sulfate to the dry powder mixer in sequence, and continue stirring for 4 minutes after the feeding is completed;
[0207] (4) Finally, add black silicate binder and white silicate binder and continue stirring for 10 minutes to obtain the fire-retardant and heat-insulating coating.
[0208] 3. Production of finishing paint
[0209] Table 6-3 Ingredients of finishing coating in Example 6
[0210] Serial number Raw material name Weight 1 diatomite 35 2 Closed-cell perlite (100 mesh) 24 3 Expanded Vermiculite (220 mesh) 100 4 Microbeads (150 mesh) 40 5 Alumina Fiber 400 6 Aluminum silicate fiber 400 7 Titanium dioxide 12 8 Zirconium-containing aluminum silicate fiber 6 9 Polyvinyl alcohol powder 5 10 Latex powder 40 11 Turquoise 0.3
[0211] The production steps of finishing layer powder are as follows:
[0212] (1) Weigh the materials in Table 6-3 according to the proportion;
[0213] (2) Start the dry powder mixer, add the measured materials in sequence, and stir for about 30 minutes to fully disperse the fibers to obtain the finishing coating.
[0214] Test Example 1
[0215] This test example discloses the performance test of the fire retardant coating of the present invention. First, the fire retardant coating of Example 1 is used to construct a sample on a steel beam, and then a performance test is performed.
[0216] 1. Sample preparation
[0217] The fire resistance test uses 36b hot-rolled I-beams specified in GB / T706-2016. The rust, oil, dust and other debris on the surface of the steel structure are removed, and then epoxy zinc-rich anti-rust paint is applied once with a thickness of about 40 to 80um, and then cured indoors for 24 hours.
[0218] Apply the interface agent evenly on the surface of the I-beam. When the interface layer is not completely dry, spray the fire retardant coating containing the interface agent (fireproof and heat-insulating coating: water: interface agent = 100:150:5, mass ratio) first, and then apply the fire retardant coating containing the interface agent to a thickness of 40mm. Finally, apply the finishing coating containing the interface agent (finishing coating: water: interface agent = 100:150:8, mass ratio) to the test thickness, and meet the specified test conditions after curing for 25 days.
[0219] 2. Testing
[0220] During the fire resistance test, four standard cover plates were placed on the upper surface of the steel beam specimen. The cover plates were made of 800kg / m 3 The lightweight concrete slab is 150mm thick, 1000mm long and 600mm wide. A layer of aluminum silicate fiber wool is set between the cover plate and the upper flange of the beam, and its width is equal to the width of the upper flange of the beam. The specimen is loaded with four-point concentrated loads (simulating uniformly distributed loads). A total of 12 thermocouples are arranged inside the steel beam. The thermocouple arrangement is as shown in the attached figure. Figure 1 As shown in the figure, the calculated span of the steel beam is 4200mm and the total external load is 207kN.
[0221] Physical and chemical properties test pieces are sampled in accordance with the requirements of GB14907-2018 "Fire Retardant Coatings for Steel Structures".
[0222] The results are shown in the following table:
[0223] Table 7 Test results
[0224]
[0225]
[0226] After the test, the steel beam was removed from the refractory furnace and its appearance was as shown in the attached figure. Figure 2 As shown in the attached figure at the end of the test, it can be seen that the non-expansion steel structure composite layer protection system of the present invention can meet the 4.0h resistance requirement.
[0227] The non-expansive steel structure composite protection system of the invention is compared with the inspection reports of non-expansive steel structure fire retardant coatings produced by major fire retardant coating representative manufacturers in the prior art, and the results are as follows:
[0228] Table 8 Technical index analysis of non-expansive steel structure fire retardant coating
[0229]
[0230] From the above table, we can see that it has the following characteristics:
[0231] (1) The fire resistance limit of non-expanding steel structure fire retardant coating reaches 4.0h, and the thickness of the fire retardant coating needs to reach or exceed 40mm.
[0232] (2) The composite fire protection technology of the present invention provides a composite fire protection system in which the internal temperature of the steel beam is less than 400°C for 4 hours, showing excellent thermal insulation performance.
[0233] (3) Judging from the maximum bending deformation at the end of the test, the deformation of the multi-layer fire protection system is lower than that of its peers.
[0234] (4) Number of cracks at the end point of the test: the composite fire protection system has the least cracks.
[0235] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.
Claims
1. A non-expanding fire retardant coating for steel structures, characterized in that: Including interface agent, fire-retardant and heat-insulating coating powder and finishing material coating.
2. A non-expanding fire retardant coating for steel structures according to claim 1, characterized in that: The interface agent is made of the following raw materials in parts by weight: 90520-80 parts of flame retardant emulsion, 15-70 parts of solid mixture, 121-4 parts of alcohol ester, 11-44 parts of glass microspheres, 0.05-0.2 parts of hydroxyethyl cellulose, and 10-60 parts of water; Preferably, the interface agent is made of raw materials including the following parts by weight: 90550-60 parts of flame retardant emulsion, 25-45 parts of solid mixture, 121-3 parts of alcohol ester, 14-30 glass microspheres, 0.08-0.12 parts of hydroxyethyl cellulose, and 10-45 parts of water.
3. The non-expanding fire retardant coating for steel structures according to claim 1, characterized in that: The solid mixture is composed of silicon micropowder, silicon carbide powder and attapulgite powder in a mass ratio of 4-16:0.5-2:0.05-0.2; Preferably, the solid mixture is composed of silicon micropowder, silicon carbide powder and attapulgite powder in a mass ratio of 6-12:0.8-1.2:0.08-0.
12.
4. The non-expanding fire retardant coating for steel structures according to claim 1, characterized in that: The fireproof and heat-insulating coating powder is made of the following raw materials in parts by weight: 450-1800 parts of black silicate binder, 90-360 parts of white silicate binder, 75-300 parts of expanded perlite, 425-1700 parts of expanded vermiculite, 10-40 parts of floating beads, 110-440 parts of mica, 1.5-6 parts of hydroxypropyl cellulose, 0.1-0.4 parts of sodium lauryl sulfate, 2-8 parts of zirconium-containing aluminum silicate fiber, and 25-100 parts of alumina fiber; Preferably, the fireproof and heat-insulating coating powder is made of raw materials including the following parts by weight: 600-1200 parts of black silicate binder, 150-210 parts of white silicate binder, 100-200 parts of expanded perlite, 700-1000 parts of expanded vermiculite, 15-25 parts of floating beads, 180-250 parts of mica, 2-4 parts of hydroxypropyl cellulose, 0.1-0.3 parts of sodium lauryl sulfate, 3-5 parts of zirconium-containing aluminum silicate fiber, and 40-60 parts of alumina fiber.
5. The non-expanding fire retardant coating for steel structures according to claim 1, characterized in that: The finishing paint is made of the following raw materials in parts by weight: 10-40 parts of diatomaceous earth, 6-24 parts of closed-cell perlite, 40-160 parts of expanded vermiculite, 10-40 parts of microspheres, 100-400 parts of alumina fiber, 250-1000 parts of aluminum silicate fiber, 5-20 parts of titanium dioxide, 2-8 parts of zirconium-containing aluminum silicate fiber, 1.5-6 parts of polyvinyl alcohol powder, 15-60 parts of latex powder, and 0.1-0.4 parts of turquoise blue; Preferably, the finishing paint is made of raw materials including the following parts by weight: 10-30 parts of diatomaceous earth, 8-16 parts of closed-cell perlite, 60-100 parts of expanded vermiculite, 10-30 parts of microspheres, 10-300 parts of alumina fiber, 400-600 parts of aluminum silicate fiber, 8-12 parts of titanium dioxide, 2-6 parts of zirconium-containing aluminum silicate fiber, 2-5 parts of polyvinyl alcohol powder, 20-40 parts of latex powder, and 0.15-0.3 parts of turquoise blue.
6. The non-expanding fire retardant coating for steel structures according to claim 1, characterized in that: The interface agent is made of the following raw materials in parts by weight: 90540 parts of flame retardant emulsion, 35 parts of solid mixture, 122 parts of alcohol ester, 22 parts of glass microspheres, 0.1 parts of hydroxyethyl cellulose, and 20-30 parts of water; the solid mixture is composed of silicon micropowder: silicon carbide powder: attapulgite powder in a mass ratio of 8:1:0.1; The fireproof and heat-insulating coating powder is made of the following raw materials in parts by weight: 900 parts of black silicate binder, 180 parts of white silicate binder, 150 parts of expanded perlite, 850 parts of expanded vermiculite, 20 parts of floating beads, 220 parts of mica, 3 parts of hydroxypropyl cellulose, 0.2 parts of sodium lauryl sulfate, 4 parts of zirconium-containing aluminum silicate fiber, and 50 parts of alumina fiber; The finishing paint is made of raw materials including the following parts by weight: 20 parts of diatomaceous earth, 12 parts of closed-cell perlite, 80 parts of expanded vermiculite, 20 parts of microspheres, 200 parts of alumina fiber, 500 parts of aluminum silicate fiber, 10 parts of titanium dioxide, 4 parts of zirconium-containing aluminum silicate fiber, 3 parts of polyvinyl alcohol powder, 30 parts of latex powder, and 0.2 parts of turquoise blue.
7. A non-expanding fire retardant coating for steel structures according to any one of claims 1 to 6, characterized in that: The particle size of the closed-cell perlite is 80-120 mesh, preferably 100 mesh; Or / and the particle size of expanded vermiculite is 180-220 mesh, preferably 200 mesh; The particle size of the microbeads is 120-180 mesh, preferably 150 mesh.
8. A method for preparing a non-expanding fire retardant coating for steel structures according to any one of claims 1 to 7, characterized in that: The steps include: Preparation of interface agent: prepare various raw materials of interface agent in proportion and mix them evenly; Preparation of fireproof and heat-insulating coating: prepare various raw materials of fireproof and heat-insulating coating in proportion, mix them evenly, and obtain the coating; Preparation of finishing material coating: prepare various raw materials of finishing material coating according to proportion, mix well and you have it.
9. Use of a non-expanding steel structure fire retardant coating as claimed in any one of claims 1 to 7 in the preparation of a non-expanding steel structure multi-layer protection system.
10. A non-expansion steel structure composite protection system, characterized in that: Made of a non-expanding steel structure fire retardant coating as claimed in any one of claims 1 to 7, comprising an interface layer, a fire retardant and heat insulating coating layer and a finishing coating layer; Among them, the interface layer is formed by evenly coating the interface agent on the surface of the steel structure; the fireproof and heat-insulating coating layer is formed by applying the fireproof and heat-insulating coating containing the interface agent; the finishing coating layer is formed by applying the finishing coating containing the interface agent; Preferably, the fire retardant coating containing the interface agent is a mixture of fire retardant and heat insulating coating, water, and the interface agent in a mass ratio of 80 to 120:13 to 170:3 to 8, more preferably fire retardant and heat insulating coating: water: interface agent = 100:150:5; Preferably, the finishing paint containing the interface agent is a mixture of finishing paint, water and interface agent in a mass ratio of 80-120:13-170:6-10, more preferably finishing paint: water: interface agent = 100:150:8.
Citation Information
Patent Citations
Masonry binder for steel structure containment system
CN102942344A
Graphene oxide modified fireproof antiseptic dual-functional coating and method for non-expanding steel structure
CN105693153A
Non-intumescent fireproof coating for steel structure and preparation method of non-intumescent fireproof coating
CN114181554A
Fireproof structure of steel column in severe cold area
CN117248644A
Non expansion type steel structure fire retarding anticorrosion paint
CN1948404A