Yellow-resistant, antibacterial and wear-resistant sealant and preparation method thereof
By using polyasparticle and other components in the seam-beautifier to form a crosslinking network, the problem of cracking and insufficient yellowing resistance in long-term use of the seam-beautifier is solved, and good antibacterial, wear-resistant and yellowing resistance is achieved. performance.
Patent Information
- Application Number
- CN202411350900.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing seam-applied agents are prone to cracking and impurities during long-term use, which affects their antibacterial properties and wear resistance, and their yellowing resistance has not been improved.
Using polyaspartic acid ester, epoxy nanosilica, silicate cement, sulfur-containing antibacterial agent, sodium sulfonate modified silane, calcium carbonate, defoaming agent BYK088, leveling agent BYK-3060 and other components, through Specific preparation methods form crosslinking networks to improve antibacterial, wear and yellowing resistance.
It significantly improves the antibacterial properties, wear resistance and yellowing resistance of the seam-applied agent, ensuring that it is not prone to cracking and discoloration during long-term use.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of seam beautifying agents, in particular to a yellowing-resistant, antibacterial and wear-resistant seam beautifying agent and a preparation method thereof. Background Art
[0002] Seam beautifier is a product that beautifies the gaps between wall and floor tiles. It is widely used in the decoration of gaps in materials such as stone, wood, and glass. However, during long-term use, seam beautifiers are prone to cracking and impurities, which can produce bacteria and affect their normal use. Therefore, how to avoid this phenomenon is the key to solving the problem. For example, patent CN113292959B discloses an antibacterial and antifouling seam beautifier and its preparation method. The antibacterial and antifouling seam beautifier of the invention is a solvent-free two-component seam beautifier, which is environmentally friendly and non-toxic, simple and convenient to use; it has good mechanical properties, antifouling and mildew and antibacterial properties; but its wear resistance and yellowing resistance are not improved. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies in the prior art, the present invention provides a yellowing-resistant, antibacterial and wear-resistant seam beautifying agent and a preparation method thereof, which has good yellowing-resistant, antibacterial and wear-resistant effects.
[0005] (II) Technical solution
[0006] To achieve the above objectives, the present invention provides the following technical solution: a yellowing-resistant, antibacterial and wear-resistant seam beautifying agent, comprising the following components by weight: 2-5 parts by weight of polyaspartic acid ester, 3-6 parts by weight of epoxy nano-silica, 15-25 parts by weight of silicate cement, 4-6 parts by weight of sulfur-containing antibacterial agent, 3-5 parts by weight of sodium sulfonate modified silane, 1-3 parts by weight of calcium carbonate, 0.8-1.4 parts by weight of defoamer BYK088, and 1-2 parts by weight of leveling agent BYK-3060.
[0007] Preferably, the preparation method of the sulfur-containing antibacterial agent is:
[0008] (1) Add methyldichlorosilane and 2-hydroxybenzimidazole to toluene solvent, stir and disperse, heat to 75-90°C and reflux for 7-12 hours, cool to room temperature, filter, wash and dry to obtain imidazole-modified silane;
[0009] (2) Under a nitrogen atmosphere, propylene mercaptan is dispersed in a flask filled with toluene solvent, and tris(triphenylphosphine)rhodium chloride and imidazole-modified silane are added thereto, stirred and dispersed, and an addition reaction is carried out. The temperature is raised to 95-100° C., and the reaction is refluxed for 6-12 hours. After the reaction, the mixture is distilled under reduced pressure and dried to obtain mercaptosilane;
[0010] (3) Add tetrahydrofuran solvent, allyl glycidyl ether and chloroplatinic acid catalyst into a three-necked flask, place in an oil bath at 45-55°C for 25-30 minutes, add 1,1,3,3-tetramethyldisiloxane dropwise with stirring for 40-60 minutes, stir, and continue to react at 45-50°C for 4-5 hours. After reaction, cool and then add activated carbon adsorbent, ultrasonically vibrate for 25-40 minutes, remove chloroplatinic acid catalyst, filter, and rotary evaporate to obtain an intermediate;
[0011] (4) Add the intermediate, thiol silane and tetrabutylammonium fluoride catalyst into a reactor filled with N,N-dimethylformamide solvent, and carry out a ring-opening reaction at 70-85° C. for 8-12 hours. After completion, cool, filter the solvent, and wash with ethanol to obtain an imidazole-based antibacterial agent.
[0012] Preferably, the mass ratio of methyldichlorosilane to 2-hydroxybenzimidazole in (1) is 1:2.1-2.4.
[0013] Preferably, the mass ratio of propylene mercaptan, tris(triphenylphosphine)rhodium chloride and imidazole-modified silane in (2) is 1.1-1.3:0.01-0.03:1.
[0014] Preferably, the mass ratio of allyl glycidyl ether, chloroplatinic acid catalyst and 1,1,3,3-tetramethyldisiloxane in (3) is 1:0.02-0.03:1.2-1.3.
[0015] Preferably, the mass ratio of the intermediate, thiol silane and tetrabutylammonium fluoride catalyst in (4) is 1:0.8-1.3:0.01-0.03.
[0016] Preferably, the preparation method of the sodium sulfonate modified silane is: add 6-10 parts by weight of imidazole-modified silane and 7-15 parts by weight of sodium 3-chloro-2-hydroxypropanesulfonate to N,N-dimethylformamide solvent, stir and disperse, heat to 75-90°C and react for 6-10 hours, then perform reduced pressure distillation, wash and dry to obtain sodium sulfonate modified silane.
[0017] Preferably, the preparation method of the yellowing-resistant, antibacterial and wear-resistant seam beautifying agent is: adding polyaspartic acid ester, epoxy nano-silica, silicate cement, sulfur-containing antibacterial agent, sodium sulfonate modified silane, calcium carbonate, defoaming agent BYK088, and leveling agent BYK-3060 into a reactor, stirring for 5-10 minutes, and rotating at a speed of 700-850r / min to obtain the yellowing-resistant, antibacterial and wear-resistant seam beautifying agent.
[0018] 3. Beneficial technical effects
[0019] The invention prepares a yellowing-resistant, antibacterial and wear-resistant seam beautifying agent by adding polyaspartic acid ester, epoxy nano-silicon dioxide, silicate cement, sulfur-containing antibacterial agent, sodium sulfonate-modified silane, calcium carbonate, defoamer BYK088 and leveling agent BYK-3060 into a reactor and stirring the mixture.
[0020] The imidazole group and the sodium sulfonate group in the sulfur-containing antibacterial agent and the sodium sulfonate modified silane have good antibacterial effect, and are applied in the seam beautifying agent to improve its antibacterial performance; during the stirring process, the epoxy nano-silica will undergo a ring-opening reaction with the hydroxyl groups in the sulfur-containing antibacterial agent and the sodium sulfonate modified silane, so that they are more closely connected to each other, forming a cross-linked network, and improving its wear resistance; the sulfur element, nitrogen element, and siloxane in the seam beautifying agent will form hydrogen bonds to form a network, which also increases its wear resistance; the seam beautifying agent of the present invention also has good yellowing resistance. DETAILED DESCRIPTION
[0021] The preparation method of epoxy nano-silica is based on the article "Silane coupling agent KH-560 modified nano-silica" in the 8th issue of Vol. 3 of Chemical World in August 2011. 2 Add 20 mL of toluene and use a KQ-300E ultrasonic cleaner (300 W) for ultrasonic dispersion at room temperature for 30 minutes to obtain a uniform suspension, then add silane coupling agent KH-560 and continue ultrasonic dispersion for 3-4 minutes, transfer to a 100 mL four-necked flask equipped with a reflux condenser and a power-enhanced electric stirrer, and stir in an oil bath at a set temperature for reaction. The slurry after the reaction is centrifuged at room temperature at a speed of 12000 r / min using a CT15RT desktop high-speed refrigerated centrifuge to obtain epoxy nano-silica.
[0022] Example 1
[0023] (1) adding methyldichlorosilane and 2-hydroxybenzimidazole into toluene solvent, wherein the mass ratio of methyldichlorosilane to 2-hydroxybenzimidazole is 1:2.1, stirring and dispersing, heating to 75° C. and reflux reaction for 7 h, cooling to room temperature after reaction, filtering, washing, and drying to obtain imidazole-modified silane;
[0024] (2) Under a nitrogen atmosphere, propylene mercaptan is dispersed in a flask filled with toluene solvent, and tris(triphenylphosphine)rhodium chloride and imidazole-modified silane are added thereto, wherein the mass ratio of propylene mercaptan, tris(triphenylphosphine)rhodium chloride and imidazole-modified silane is 1.1:0.01:1, and the mixture is dispersed by stirring to carry out an addition reaction, and the temperature is raised to 95° C., and the mixture is refluxed for 6 hours. After the reaction, the mixture is distilled under reduced pressure and dried to obtain thiol silane;
[0025] (3) Add tetrahydrofuran solvent, allyl glycidyl ether and chloroplatinic acid catalyst into a three-necked flask, place in an oil bath at 45°C for 25 minutes, add 1,1,3,3-tetramethyldisiloxane dropwise with stirring, wherein the mass ratio of allyl glycidyl ether, chloroplatinic acid catalyst and 1,1,3,3-tetramethyldisiloxane is 1:0.02:1.2, and the addition time is 40 minutes. Stir and continue to react at 45°C for 4 hours. After the reaction is completed, cool and then add activated carbon adsorbent, ultrasonically shake for 25 minutes, remove the chloroplatinic acid catalyst, filter and rotary evaporate to obtain an intermediate;
[0026] (4) adding the intermediate, thiol silane and tetrabutylammonium fluoride catalyst into a reactor filled with N,N-dimethylformamide solvent, wherein the mass ratio of the intermediate, thiol silane and tetrabutylammonium fluoride catalyst is 1:0.8:0.01, and performing a ring-opening reaction at 70°C for 8 hours. After completion, cooling, filtering the solvent, and washing with ethanol to obtain an imidazole-based antibacterial agent;
[0027] (5) adding 6 parts by weight of imidazole-modified silane and 7 parts by weight of sodium 3-chloro-2-hydroxypropanesulfonate to N,N-dimethylformamide solvent, stirring and dispersing, heating to 75° C. and reacting for 6 hours, and then distilling under reduced pressure, washing and drying to obtain sodium sulfonate-modified silane;
[0028] (6) Add 2 parts by weight of polyaspartic acid ester, 3 parts by weight of epoxy nano-silica, 15 parts by weight of silicate cement, 4 parts by weight of sulfur-containing antibacterial agent, 3 parts by weight of sodium sulfonate modified silane, 1 part by weight of calcium carbonate, 0.8 parts by weight of defoaming agent BYK088, and 1 part by weight of leveling agent BYK-3060 into the reactor, stir for 5 minutes, and increase the speed to 700 r / min to obtain a yellowing-resistant, antibacterial and wear-resistant seam beautifying agent.
[0029] Example 2
[0030] (1) adding methyldichlorosilane and 2-hydroxybenzimidazole into toluene solvent, wherein the mass ratio of methyldichlorosilane to 2-hydroxybenzimidazole is 1:2.4, stirring and dispersing, heating to 90° C. and reflux reaction for 12 h, cooling to room temperature after reaction, filtering, washing, and drying to obtain imidazole-modified silane;
[0031] (2) Under a nitrogen atmosphere, propylene mercaptan is dispersed in a flask filled with toluene solvent, and tris(triphenylphosphine)rhodium chloride and imidazole-modified silane are added thereto, wherein the mass ratio of propylene mercaptan, tris(triphenylphosphine)rhodium chloride and imidazole-modified silane is 1.3:0.03:1, the mixture is dispersed by stirring, and an addition reaction is carried out. The mixture is heated to 100° C. and refluxed for 12 hours. After the reaction, the mixture is distilled under reduced pressure and dried to obtain thiol silane;
[0032] (3) Add tetrahydrofuran solvent, allyl glycidyl ether and chloroplatinic acid catalyst into a three-necked flask, place in an oil bath at 55°C for 30 minutes, add 1,1,3,3-tetramethyldisiloxane dropwise with stirring, wherein the mass ratio of allyl glycidyl ether, chloroplatinic acid catalyst and 1,1,3,3-tetramethyldisiloxane is 1:0.03:1.3, and the addition time is 60 minutes. Stir and continue to react at 50°C for 5 hours. After the reaction is completed, cool and then add activated carbon adsorbent, ultrasonically shake for 40 minutes, remove the chloroplatinic acid catalyst, filter and rotary evaporate to obtain an intermediate;
[0033] (4) adding the intermediate, thiol silane and tetrabutylammonium fluoride catalyst into a reactor filled with N,N-dimethylformamide solvent, wherein the mass ratio of the intermediate, thiol silane and tetrabutylammonium fluoride catalyst is 1:1.3:0.03, and performing a ring-opening reaction at 85°C for 12 hours. After completion, cooling, filtering the solvent, and washing with ethanol to obtain an imidazole-based antibacterial agent;
[0034] (5) adding 10 parts by weight of imidazole-modified silane and 15 parts by weight of sodium 3-chloro-2-hydroxypropanesulfonate to N,N-dimethylformamide solvent, stirring and dispersing, heating to 90° C. and reacting for 10 hours, and then distilling under reduced pressure, washing and drying to obtain sodium sulfonate-modified silane;
[0035] (6) Add 5 parts by weight of polyaspartic acid ester, 6 parts by weight of epoxy nano-silica, 25 parts by weight of silicate cement, 6 parts by weight of sulfur-containing antibacterial agent, 5 parts by weight of sodium sulfonate modified silane, 3 parts by weight of calcium carbonate, 1.4 parts by weight of defoaming agent BYK088, and 2 parts by weight of leveling agent BYK-3060 into the reactor, stir for 10 minutes, and increase the speed to 850 r / min to obtain a yellowing-resistant, antibacterial and wear-resistant seam beautifying agent.
[0036] Example 3
[0037] (1) adding methyldichlorosilane and 2-hydroxybenzimidazole to a toluene solvent, wherein the mass ratio of methyldichlorosilane to 2-hydroxybenzimidazole is 1:2.25, stirring and dispersing, heating to 82° C. and reflux reaction for 10 h, cooling to room temperature after reaction, filtering, washing, and drying to obtain imidazole-modified silane;
[0038] (2) Under a nitrogen atmosphere, propylene mercaptan is dispersed in a flask filled with toluene solvent, and tris(triphenylphosphine)rhodium chloride and imidazole-modified silane are added thereto, wherein the mass ratio of propylene mercaptan, tris(triphenylphosphine)rhodium chloride and imidazole-modified silane is 1.2:0.02:1, and the mixture is dispersed by stirring to carry out an addition reaction, and the temperature is raised to 97° C., and the mixture is refluxed for 9 hours. After the reaction, the mixture is distilled under reduced pressure and dried to obtain thiol silane;
[0039] (3) Add tetrahydrofuran solvent, allyl glycidyl ether and chloroplatinic acid catalyst into a three-necked flask, place in an oil bath at 50°C for 27 minutes, add 1,1,3,3-tetramethyldisiloxane dropwise with stirring, wherein the mass ratio of allyl glycidyl ether, chloroplatinic acid catalyst and 1,1,3,3-tetramethyldisiloxane is 1:0.025:1.25, and the addition time is 50 minutes. Stir and continue to react at 47°C for 4.5 hours. After the reaction is completed, cool and then add activated carbon adsorbent, ultrasonically shake for 32 minutes, remove the chloroplatinic acid catalyst, filter and rotary evaporate to obtain an intermediate;
[0040] (4) adding the intermediate, thiol silane and tetrabutylammonium fluoride catalyst into a reactor filled with N,N-dimethylformamide solvent, wherein the mass ratio of the intermediate, thiol silane and tetrabutylammonium fluoride catalyst is 1:1.1:0.02, and performing a ring-opening reaction at 82°C for 10 hours. After completion, cooling, filtering the solvent, and washing with ethanol to obtain an imidazole-based antibacterial agent;
[0041] (5) adding 8 parts by weight of imidazole-modified silane and 12 parts by weight of sodium 3-chloro-2-hydroxypropanesulfonate to N,N-dimethylformamide solvent, stirring and dispersing, heating to 80° C. and reacting for 8 hours, and then distilling under reduced pressure, washing and drying to obtain sodium sulfonate-modified silane;
[0042] (6) 3.5 parts by weight of polyaspartic acid ester, 4.5 parts by weight of epoxy nano-silica, 20 parts by weight of silicate cement, 5 parts by weight of sulfur-containing antibacterial agent, 4 parts by weight of sodium sulfonate modified silane, 2 parts by weight of calcium carbonate, 1.2 parts by weight of defoaming agent BYK088, and 1.5 parts by weight of leveling agent BYK-3060 were added to the reactor and stirred for 8 minutes at a speed of 800 r / min to obtain a yellowing-resistant, antibacterial and wear-resistant seam beautifying agent.
[0043] Comparative Example 1
[0044] This comparative example is compared with Example 3, except that no sulfur-containing antibacterial agent is added.
[0045] Comparative Example 2
[0046] The difference between this comparative example and Example 3 is that no sodium sulfonate-modified silane is added.
[0047] The antibacterial property is tested according to GB / T1741-2007 "Determination of the Antifungal Resistance of Paint Films", and the antibacterial rate is calculated. The wear resistance is tested according to JC / T1004-2017. The yellowing resistance test method is: the seam beautifying agent prepared by the present invention is naturally placed for 60 days and the appearance is observed.
[0048] Table 1: Yellowing resistance, antibacterial and anti-wear performance test.
[0049] project Antibacterial activity (%) <![CDATA[Wear resistance (mm 3 )]]> Yellowing resistance Example 1 98.2 523 No color change Example 2 99.6 517 No color change Example 3 98.4 516 No color change Comparative Example 1 92.1 1246 Slightly yellow Comparative Example 2 92.4 1219 Slightly yellow
[0050] It can be seen from Table 1 that Examples 1-3 of the present invention have better yellowing resistance, antibacterial and abrasion resistance than Comparative Examples 1-2.
[0051] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A yellowing-resistant, antibacterial and wear-resistant seam-beautifying agent, characterized in that: The invention comprises the following components by weight: 2-5 parts by weight of polyaspartic acid ester, 3-6 parts by weight of epoxy nano-silica, 15-25 parts by weight of silicate cement, 4-6 parts by weight of sulfur-containing antibacterial agent, 3-5 parts by weight of sodium sulfonate modified silane, 1-3 parts by weight of calcium carbonate, 0.8-1.4 parts by weight of defoamer BYK088 and 1-2 parts by weight of leveling agent BYK-3060.
2. The yellowing-resistant, antibacterial and wear-resistant seam-beautifying agent according to claim 1, characterized in that: The preparation method of the sulfur-containing antibacterial agent is: (1) Add methyldichlorosilane and 2-hydroxybenzimidazole to toluene solvent, stir and disperse, heat to 75-90°C and reflux for 7-12 hours, cool to room temperature, filter, wash and dry to obtain imidazole-modified silane; (2) Under a nitrogen atmosphere, propylene mercaptan is dispersed in a flask filled with toluene solvent, and tris(triphenylphosphine)rhodium chloride and imidazole-modified silane are added thereto, stirred and dispersed, and an addition reaction is carried out. The temperature is raised to 95-100° C., and the reaction is refluxed for 6-12 hours. After the reaction, the mixture is distilled under reduced pressure and dried to obtain mercaptosilane; (3) Add tetrahydrofuran solvent, allyl glycidyl ether and chloroplatinic acid catalyst into a three-necked flask, place in an oil bath at 45-55°C for 25-30 minutes, add 1,1,3,3-tetramethyldisiloxane dropwise with stirring for 40-60 minutes, stir, and continue to react at 45-50°C for 4-5 hours. After reaction, cool and then add activated carbon adsorbent, ultrasonically vibrate for 25-40 minutes, remove chloroplatinic acid catalyst, filter, and rotary evaporate to obtain an intermediate; (4) Add the intermediate, thiol silane and tetrabutylammonium fluoride catalyst into a reactor filled with N,N-dimethylformamide solvent, and carry out a ring-opening reaction at 70-85° C. for 8-12 hours. After completion, cool, filter the solvent, and wash with ethanol to obtain an imidazole-based antibacterial agent.
3. The yellowing-resistant, antibacterial and wear-resistant seam-beautifying agent according to claim 2, characterized in that: The mass ratio of methyldichlorosilane to 2-hydroxybenzimidazole in (1) is 1:2.1-2.
4.
4. The yellowing-resistant, antibacterial and wear-resistant seam-beautifying agent according to claim 2, characterized in that: The mass ratio of propylene mercaptan, tris(triphenylphosphine)rhodium chloride and imidazole-modified silane in (2) is 1.1-1.3:0.01-0.03:
1.
5. The yellowing-resistant, antibacterial and wear-resistant seam-beautifying agent according to claim 2, characterized in that: The mass ratio of allyl glycidyl ether, chloroplatinic acid catalyst and 1,1,3,3-tetramethyldisiloxane in (3) is 1:0.02-0.03:1.2-1.
3.
6. The yellowing-resistant, antibacterial and wear-resistant seam-beautifying agent according to claim 2, characterized in that: The mass ratio of the intermediate, mercaptosilane and tetrabutylammonium fluoride catalyst in (4) is 1:0.8-1.3:0.01-0.
03.
7. The yellowing-resistant, antibacterial and wear-resistant seam-beautifying agent according to claim 1, characterized in that: The preparation method of the sodium sulfonate modified silane is as follows: 6-10 parts by weight of imidazole modified silane and 7-15 parts by weight of sodium 3-chloro-2-hydroxypropanesulfonate are added to N,N-dimethylformamide solvent, stirred and dispersed, heated to 75-90° C. and reacted for 6-10 hours, and then subjected to reduced pressure distillation, washed and dried to obtain the sodium sulfonate modified silane.
8. A method for preparing the yellowing-resistant, antibacterial and anti-wear seam beautifying agent according to any one of claims 1 to 7, characterized in that: The preparation method of the yellowing-resistant, antibacterial and wear-resistant seam beautifying agent comprises the following steps: adding polyaspartic acid ester, epoxy nano-silica, silicate cement, sulfur-containing antibacterial agent, sodium sulfonate-modified silane, calcium carbonate, defoaming agent BYK088 and leveling agent BYK-3060 into a reactor, stirring for 5-10 minutes, and rotating at a speed of 700-850 r / min to obtain the yellowing-resistant, antibacterial and wear-resistant seam beautifying agent.