Fluoroether coating and preparation method thereof
The fluoroether coating addresses mold growth, reflectivity loss, and rain marks by using a specific formulation and process, enhancing weather resistance and durability.
Patent Information
- Application Number
- CN202411303938.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
AI Technical Summary
Current exterior wall coatings face issues with mold growth, reflectivity attenuation, and rain marks, which affect the visual appearance and structural integrity of buildings.
A fluoroether coating composed of specific components, including fluoroolefin-vinyl ether copolymer, titanium dioxide, silicone-modified polyacrylate, and mildew inhibitors, is formulated and prepared through a controlled process to enhance weather resistance, chemical corrosion resistance, and insulation properties.
The fluoroether coating maintains long-term stain resistance, reduces energy consumption, prevents mold, and avoids rain marks, while ensuring uniformity and durability.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, in particular to a fluoroether coating and a preparation method thereof. Background Art
[0002] Building exterior wall coatings are important materials for protecting the exterior walls of buildings. They not only beautify the appearance of buildings, but also have multiple functions such as waterproofing, anti-corrosion, and heat preservation. The current exterior wall coatings have the following problems: 1. Mold growth: In a damp and humid environment, many coatings are difficult to effectively resist the invasion of mold, resulting in frequent mold spots on the coating surface, which not only damages the visual beauty, but may also cause potential damage to the building structure, greatly shortening the service life of the coating.
[0003] 2. Reflectivity attenuation: When the paint is exposed to harsh conditions such as ultraviolet rays and rain outdoors, its surface reflectivity decreases significantly. The reduced reflectivity leads to increased heat absorption and energy consumption of the building, and also affects the maintenance of the building's appearance.
[0004] 3. Obvious rain marks: Under the action of rain, some paint surfaces are prone to form clearly visible rain marks or water stains, which not only destroys the uniformity and aesthetics of the coating, but may also accelerate the erosion process of the substrate under the coating.
[0005] Therefore, it is necessary to propose a fluoroether coating and a preparation method thereof to solve the above problems. Summary of the invention
[0006] 1. Technical issues to be resolved The object of the present invention is to provide a fluoroether coating and a preparation method thereof to solve the problems raised in the above background technology.
[0007] (II) Technical solution To achieve the above objectives, the present invention is implemented through the following technical scheme: a fluoroether coating, composed of the following components in parts by weight: 40 to 60 parts of fluoroolefin-vinyl ether copolymer, 35 to 45 parts of organic solvent, 13 to 17 parts of pigment, 8 to 15 parts of titanium dioxide, 8 to 12 parts of silicone-modified polyacrylate, 2 to 6 parts of cross-linking agent, 1 to 3 parts of auxiliary agent, and 1 to 3 parts of mildewproof agent.
[0008] Furthermore, the auxiliary agent includes a dispersant and an inhibitor.
[0009] Furthermore, the mildew inhibitor is a mixture of 2-methyl-4-isothiazoline-3-one and 5-chloro-2-methyl-4-isothiazoline-3-one, and the mixing ratio of the two is 1:(2-3).
[0010] Furthermore, the fluoroolefin-vinyl ether copolymer contains structural units represented by formula (1), formula (2) and formula (3), In formula (1), formula (2) and formula (3), X is one of F, CF3 and Cl, and R1, R2 and R3 are alkyl groups having 1 to 6 carbon atoms.
[0011] Furthermore, the particle size of the titanium dioxide is 0.1-0.3 μm.
[0012] Furthermore, it is composed of the following components in parts by weight: 50 parts of fluoroolefin-vinyl ether copolymer, 40 parts of organic solvent, 15 parts of pigment, 13 parts of titanium dioxide, 10 parts of silicone-modified polyacrylate, 4 parts of cross-linking agent, 2 parts of auxiliary agent, and 2 parts of mildewproofing agent.
[0013] A method for preparing a fluoroether coating comprises the following steps: dissolving a fluoroolefin-vinyl ether copolymer in a solvent; Adding organosilicon-modified polyacrylate and dispersant to the obtained solution, stirring and mixing, then adding pigment and silicon dioxide to the mixture for grinding, and finally adding crosslinking agent, mildew inhibitor and polymerization inhibitor to the ground material, stirring and mixing again; The temperature is controlled at 50-55°C and the product is filtered to obtain the fluoroether coating.
[0014] (III) Beneficial effects Compared with the prior art, the present invention provides a fluoroether coating and a preparation method thereof, which has the following beneficial effects: 1. The fluoroether paint has good weather resistance, chemical corrosion resistance and insulation properties. By adding titanium dioxide, the paint can maintain a long-term stain resistance effect, thereby ensuring the reflectivity of the paint, and significantly reducing the energy consumption of the building when used as an exterior wall paint; by adding mildew inhibitors, the coating can be prevented from mold in a humid environment; by adding silicone-modified polyacrylate, the paint will not leave rain marks on the exterior wall, and dust will not adhere, making it last longer.
[0015] 2. The preparation method of the fluoroether coating has a reasonable design of the entire preparation process and a moderate operating temperature, avoiding complex conditions such as high temperature and high pressure, reducing production difficulty and cost. It has good replicability and scalability, and is convenient for large-scale industrial production. DETAILED DESCRIPTION
[0016] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0017] A fluoroether coating is composed of the following components in parts by weight: 40-60 parts of fluoroolefin-vinyl ether copolymer, 35-45 parts of organic solvent, 13-17 parts of pigment, 8-15 parts of titanium dioxide, 8-12 parts of organosilicon-modified polyacrylate, 2-6 parts of crosslinking agent, 1-3 parts of auxiliary agent and 1-3 parts of mildewproof agent.
[0018] Fluoroolefin-vinyl ether copolymer, as an environmentally friendly polymer resin, has good weather resistance, chemical corrosion resistance and insulation. After adding titanium dioxide, titanium dioxide continuously decomposes organic matter accumulated on the surface of the paint under light, causing the adsorbed dust to lose the "organic adhesion" between the paint and the paint. At the same time, it has super hydrophilicity, producing a layer of water film on the surface of the paint to isolate oily pollutants from the surface. Through the above dual effects, the paint maintains a long-term stain resistance effect, thereby ensuring the reflectivity of the paint, and significantly reducing building energy consumption when used as an exterior wall paint. By adding mildew inhibitors, ensure that the coating does not mold in a humid environment. By adding silicone-modified polyacrylate, the hydrophobic properties of silicone make the modified paint have better waterproof properties, which can effectively prevent water penetration and erosion, so that the paint will not have rain marks on the exterior wall, and dust will not adhere.
[0019] The solvent is one or more of butanone, ethyl acetate, methyl isobutyl ketone, toluene, xylene, n-butanol, ethylene glycol acetate, ethylene glycol methyl ether, cyclohexanone, and ethylene glycol butyl ether. When the above solvents dissolve the fluoroolefin-vinyl ether copolymer, the apparent viscosity decreases in sequence. Preferably, the weight ratio of butyl acetate to ethylene glycol butyl ether in the solvent is 5:5 to 7. By mixing the above two raw materials, the coating has a suitable viscosity, and at the same time, it has low toxicity and low cost.
[0020] Specifically, the crosslinking agent is a mixture of blocked isocyanate and amino resin, which can react with the hydroxyl group in the copolymer to form a stable crosslinking structure, which makes the coating have higher hardness, wear resistance, weather resistance and chemical corrosion resistance. Among them, the ratio of blocked isocyanate to amino resin is 1:6-7. This ratio of crosslinking agent helps to improve the leveling of the coating and reduce the viscosity, making the coating more uniform and smooth during the construction process.
[0021] The auxiliary agent includes a dispersant and an inhibitor, wherein the dispersant is a polymer dispersant, which has a long molecular chain and more functional groups, and can wrap solid particles in the molecular chain by adsorption, bridging, etc. to form a stable dispersion system, such as polyacrylates and polymaleic anhydride / octadecyl ester copolymers; the inhibitor is added to avoid gelation during the storage of the coating, such as phenol and hydroquinone, which react with free radicals to generate non-free radical substances or low-activity free radicals, thereby inhibiting the polymerization reaction. Specifically, the dispersant is sodium polyacrylate and the inhibitor is hydroquinone.
[0022] Specifically, the mildew preventer is a mixture of 2-methyl-4-isothiazoline-3-one and 5-chloro-2-methyl-4-isothiazoline-3-one, with the mixing ratio of the two being 1:(2-3). It has good chemical stability, is not easy to decompose, can maintain its mildew preventive effect in the coating for a long time, and is not easy to produce harmful substances during use.
[0023] In some embodiments, the fluoroolefin-vinyl ether copolymer contains structural units represented by formula (1), formula (2) and formula (3), In formula (1), formula (2) and formula (3), X is one of F, CF3 and Cl, and R1, R2 and R3 are alkyl groups with carbon numbers of 1 to 6. Among them, R1 helps to improve its solvent solubility, improve the flexibility and glossiness of the coating, and also helps to improve the hardness of the coating. R2OH helps to improve its adhesion to the substrate, ensures a firm bond between the coating and the substrate, and enhances the durability and service life of the coating. R3COOH helps to promote the dispersion of the pigment in the coating system, improves the uniformity and stability of the pigment, and further enhances the adhesion of the coating.
[0024] Specifically, the particle size of the titanium dioxide is 0.1-0.3 μm. By using titanium dioxide with this particle size, it can be dispersed more evenly in the coating, providing more uniform and effective ultraviolet shielding, and reducing the damage of ultraviolet rays to the substrate.
[0025] Example 1 Dissolve 50 parts of fluoroolefin-vinyl ether copolymer in 40 parts of solvent; 10 parts of organosilicon-modified polyacrylate and 1 part of dispersant are added to the obtained polymer solution, and the mixture is mixed by a stirrer, and the rotation speed is controlled at 500 rpm. Then, 5 parts of pigment and 13 parts of silicon dioxide are added to the mixture, and the mixture is ground by a ball mill, and the rotation speed is controlled at 90 rpm. Finally, 4 parts of cross-linking agent, 2 parts of mildewproof agent and 1 part of polymerization inhibitor are added to the ground material, and the mixture is stirred and mixed again by a stirrer, and the rotation speed is controlled at 300 rpm. The temperature is controlled at 50-55° C. and the mixture is filtered to obtain a fluoroether coating after filtration.
[0026] Among them, the filtering form adopts filter element filtration or filter bag filtration, and the temperature is controlled at 50-55°C during filtration to reduce the viscosity of the paint, thereby achieving the purpose of improving the filtering effect.
[0027] Example 2 Dissolve 40 parts of fluoroolefin-vinyl ether copolymer in 35 parts of solvent; 8 parts of organosilicon-modified polyacrylate and 1 part of dispersant are added to the obtained polymer solution, and the mixture is mixed by a stirrer, and the rotation speed is controlled at 500 rpm. Then, 13 parts of pigment and 8 parts of silicon dioxide are added to the mixture, and the mixture is ground by a ball mill, and the rotation speed is controlled at 90 rpm. Finally, 2 parts of a cross-linking agent, 1 part of a mildew preventer and 1 part of an inhibitor are added to the ground material, and the mixture is stirred and mixed again by a stirrer, and the rotation speed is controlled at 300 rpm. The temperature is controlled at 50-55° C. and the mixture is filtered to obtain a fluoroether coating after filtration.
[0028] Example 3 Dissolve 60 parts of fluoroolefin-vinyl ether copolymer in 45 parts of solvent; 8 parts of organosilicon-modified polyacrylate and 1.5 parts of dispersant are added to the obtained polymer solution, and the mixture is mixed by a stirrer, and the rotation speed is controlled to be 500 rpm. Then, 17 parts of pigment and 15 parts of silicon dioxide are added to the mixture, and the mixture is ground by a ball mill, and the rotation speed is controlled to be 90 rpm. Finally, 6 parts of cross-linking agent, 3 parts of mildewproof agent and 1.5 parts of polymerization inhibitor are added to the ground material, and the mixture is stirred and mixed again by a stirrer, and the rotation speed is controlled to be 300 rpm. The temperature is controlled at 50-55° C. and the mixture is filtered, and a fluoroether coating is obtained after filtration.
[0029] It can be seen from the above results that the fluoroether coating provided by the present invention has excellent UV resistance, acid resistance, alkali resistance and bacteria resistance, and also has good adhesion.
[0030] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A fluoroether coating, characterized in that: The invention is composed of the following components in parts by weight: 40-60 parts of fluoroolefin-vinyl ether copolymer, 35-45 parts of organic solvent, 13-17 parts of pigment, 8-15 parts of titanium dioxide, 8-12 parts of organosilicon-modified polyacrylate, 2-6 parts of crosslinking agent, 1-3 parts of auxiliary agent and 1-3 parts of mildewproof agent.
2. A fluoroether coating according to claim 1, characterized in that: The auxiliary agent includes a dispersant and an inhibitor.
3. A fluoroether coating according to claim 1, characterized in that: The mildew preventer is a mixture of 2-methyl-4-isothiazoline-3-one and 5-chloro-2-methyl-4-isothiazoline-3-one, and the mixing ratio of the two is 1: (2-3).
4. A fluoroether coating according to claim 1, characterized in that: The fluoroolefin-vinyl ether copolymer contains structural units represented by formula (1), formula (2) and formula (3), In formula (1), formula (2) and formula (3), X is one of F, CF3 and Cl, and R1, R2 and R3 are alkyl groups having 1 to 6 carbon atoms.
5. A fluoroether coating according to claim 1, characterized in that: The particle size of the titanium dioxide is 0.1-0.3 μm.
6. A fluoroether coating according to claim 1, characterized in that: The invention is composed of the following components in parts by weight: 50 parts of fluoroolefin-vinyl ether copolymer, 40 parts of organic solvent, 15 parts of pigment, 13 parts of titanium dioxide, 10 parts of organosilicon-modified polyacrylate, 4 parts of crosslinking agent, 2 parts of auxiliary agent and 2 parts of mildewproof agent.
7. The method for preparing the fluoroether coating according to claim 1, characterized in that: The following steps are involved: dissolving a fluoroolefin-vinyl ether copolymer in a solvent; Adding organosilicon-modified polyacrylate and dispersant to the obtained solution, stirring and mixing, then adding pigment and silicon dioxide to the mixture for grinding, and finally adding crosslinking agent, mildew inhibitor and polymerization inhibitor to the ground material, stirring and mixing again; The temperature is controlled at 50-55°C and the product is filtered to obtain the fluoroether coating.