Laminated reflective film, reflective heat-insulating film thereof and preparation method of reflective heat-insulating film
Through the combination of stacked reflective film technology and nano-thermal insulation, a reflective insulation film without metal materials was designed, which solved the problem of insufficient signal shielding and mechanical properties of the existing glass window film, and achieved efficient infrared light reflection and energy saving Effect.
Patent Information
- Application Number
- CN202411387077.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
AI Technical Summary
The thermal insulation effect of existing automotive and architectural glass window films relies on metal doping, resulting in signal shielding problems. At the same time, high-function glass window films have shortcomings in mechanical properties and comprehensive application performance.
Using the laminated reflective film technology, the resin overlapping layer formed by overlapping different resins is used to control the reflection and transmission wavelengths by using the interference effect, combined with nano-thermal insulation agent, a reflective insulation film without metal materials is designed to realize infrared light reflection. And a wear-resistant layer, an ultraviolet barrier pressure-sensitive adhesive layer and a release film are added to the structure.
It realizes high visible light transmission and near-infrared reflection, avoids signal shielding, which not only saves energy and reduces consumption, but also improves the mechanical properties and convenience of use of the film.
Smart Images

Figure CN119060647A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass film pasting, and in particular to a laminated reflective film and a reflective heat-insulating film and a preparation method thereof. Background Art
[0002] As the new energy vehicle market and industrial chain have gradually matured in recent years, more and more competitive models have been launched, and matching window films have also come into being. However, the heat insulation effect of car window films basically comes from the doping of metals in the film layer, but metal doping often has the disadvantage of shielding signals.
[0003] Secondly, the development of high-function architectural glass window film products is also relatively rapid, especially those focusing on energy saving, safety, and environmental protection. New requirements are constantly being put forward for the comprehensive application performance of architectural glass window film products. How to design a glass film with good thermal insulation and mechanical properties is crucial. Summary of the invention
[0004] The purpose of the present invention is to provide a laminated reflective film and a reflective insulation film and a preparation method thereof, which are added with a combination of a reflective film substrate and a nano-insulating agent; at the same time, the reflective film is configured in a laminated manner without any metal materials, and the thickness control and lamination technology generated by the overlap of different resins can be used to freely control the reflection and transmission wavelengths to achieve infrared light reflection performance; it is suitable for both architectural window films and the currently popular smart cars, and there is no metal material in the structure, completely avoiding the presence of metal substances that can affect or shield signals.
[0005] The above technical objectives of the present invention are achieved through the following technical solutions:
[0006] The present invention provides a laminated reflective film, which is a resin laminated layer formed by overlapping different resins;
[0007] The resin overlapping layer includes a resin A layer and a resin B layer,
[0008] The number of layers of the resin overlapped layer is 100 to 300;
[0009] According to the adjustment of the thickness of the resin A layer and the thickness of the resin B layer, an interference reaction is generated to reflect light of different wavelengths in sunlight;
[0010] The thickness of the resin A layer and the thickness of the resin B layer are determined by the following formula:
[0011]
[0012] Where h1 and h2 are the thickness of resin A layer and resin B layer, respectively, in nm;
[0013] γ1 and γ2 are the refractive indices of resin A layer and resin B layer, respectively;
[0014] a is the adjustment coefficient, the unit is 1;
[0015] The thickness of the laminated reflective film is 10 to 200 μm.
[0016] Furthermore, the thickness of the resin A layer is 90 to 100 nm.
[0017] Further, the a is determined according to the reflected infrared wavelength;
[0018] The resin A contains polyethylene terephthalate or polyethylene naphthalate; the resin B is naphthenic acid copolymer polyester;
[0019] The refractive index of the resin A layer is 1.655 to 1.70, and the refractive index of the resin B layer is 1.68 to 1.72.
[0020] Furthermore, the reflective heat-insulating film comprises, in sequence: a wear-resistant layer, a laminated reflective film, a functional layer, a UV-blocking pressure-sensitive adhesive layer and a release film;
[0021] Wherein, the functional layer is 0 to 5 layers;
[0022] Wherein, the functional layer includes a nano thermal insulation layer and a base film.
[0023] Furthermore, the base film is a transparent polyester film or a laminated reflective film.
[0024] Furthermore, the total thickness of the reflective thermal insulation film is 53-556 μm.
[0025] Furthermore, the thickness of the laminated reflective film is 12 to 188 μm.
[0026] Furthermore, the thickness of the nano heat-insulating layer is 3 to 30 μm.
[0027] Furthermore, the nano thermal insulation layer includes the following components: an adhesive, a curing agent, a thermal insulation material, a solvent and an ultraviolet blocking agent.
[0028] The present invention also provides a method for preparing a reflective thermal insulation film, comprising the following steps:
[0029] On one surface of the laminated reflective film, a mixed material for forming a wear-resistant layer is coated, and the wear-resistant layer is obtained after drying at a temperature of 70 to 130° C. and curing with ultraviolet light;
[0030] The mixed material of the UV-blocking pressure-sensitive adhesive layer is coated on the other surface of the laminated reflective film, and the mixed material is placed at a temperature of 90 to 150° C. for 40 to 120 seconds and then cured to obtain the UV-blocking pressure-sensitive adhesive layer;
[0031] Compounding the surface of the base film of the functional layer on the side of the UV blocking pressure-sensitive adhesive layer away from the laminated reflective film;
[0032] A release film is compounded on the surface of the nano heat-insulating layer of the functional layer to obtain a reflective heat-insulating film in which each layer is compounded into one.
[0033] In summary, the present invention has the following beneficial effects:
[0034] The reflective thermal insulation film provided by the present invention has a composite structure, and each layer has a synergistic effect; the film achieves high visible light transmittance, high near-infrared reflection, and does not shield communication signals. It can not only reflect the heat radiated by the sun through the glass in summer, but also block the energy loss through heat radiation and heat conduction in winter heating, thereby achieving the purpose of energy saving and consumption reduction; in addition, the preparation method of the thermal insulation film of the present invention is simple and easy to operate, the layers are firmly combined, and it is very convenient to use. When using it, after peeling off the outermost release film, it can be directly pasted to the position where the film is needed. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 A schematic diagram of the structure of the reflective thermal insulation film provided by the present invention;
[0037] Figure 2 This is a schematic diagram of the structure of the resin overlapping layer of Example 1;
[0038] Figure 3 This is a schematic diagram of the structure of the resin overlapping layer of Example 2;
[0039] Figure 4 Schematic diagram of the structure of the resin overlapping layer of Example 3
[0040] Figure 5 Schematic diagram of the arrangement of the protrusions in the resin overlapping layer of Example 3.
[0041] Reference numerals: wear-resistant layer 1 , laminated reflective film 2 - 1 , nano heat-insulating layer 3 , base film 2 - 2 , UV-blocking pressure-sensitive adhesive layer 4 , release film 5 , resin A layer 6 , protrusion 61 , resin B layer 7 . DETAILED DESCRIPTION
[0042] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, a laminated reflective film and a reflective thermal insulation film and a preparation method thereof proposed in accordance with the present invention, their specific implementation methods, characteristics and effects are described in detail as follows.
[0043] This specific embodiment provides a laminated reflective film, characterized in that the laminated reflective film is a resin laminated layer formed by overlapping different resins;
[0044] The resin overlapping layer includes a resin A layer and a resin B layer,
[0045] The number of layers of the resin overlapped layer is 100 to 300;
[0046] According to the adjustment of the thickness of the resin A layer and the thickness of the resin B layer, an interference reaction is generated to reflect light of different wavelengths in sunlight;
[0047] The thickness of the resin A layer and the thickness of the resin B layer are determined by the following formula:
[0048]
[0049] Where h1 and h2 are the thickness of resin A layer and resin B layer, respectively, in nm;
[0050] γ1 and γ2 are the refractive indices of resin A layer and resin B layer, respectively;
[0051] a is the adjustment coefficient, the unit is 1;
[0052] The thickness of the laminated reflective film is 10 to 200 μm.
[0053] In some preferred embodiments, the thickness of the resin A layer is 90-100 nm.
[0054] In some preferred embodiments, a is determined based on the reflected infrared wavelength;
[0055] The resin A contains polyethylene terephthalate or polyethylene naphthalate; the resin B is naphthenic acid copolymer polyester;
[0056] The refractive index of the resin A layer is 1.655 to 1.70, and the refractive index of the resin B layer is 1.68 to 1.72.
[0057] It can be understood that in this embodiment, by alternately stacking different layers of resin A and resin B, adjusting their thicknesses h1 and h2, and utilizing the interference effect, the reflective film can effectively reflect light of different wavelengths in sunlight. This means that it can reflect light in a wide spectrum, including visible light, infrared light, and even part of ultraviolet light.
[0058] According to the thin film interference principle, when the optical path difference of different layers meets the interference condition, the reflected light waves will be phase superimposed, thereby enhancing the reflectivity. This specific embodiment adjusts the thickness of the resin A and resin B layers to make light of different wavelengths produce a strong interference effect in the film layer, thereby achieving higher reflection efficiency.
[0059] The a in the formula is an adjustment coefficient, which can be used to adjust the film layer according to specific optical requirements. By changing a, the optical properties of the reflective film can be flexibly controlled and the reflection ratio of light in different bands can be accurately adjusted. This flexibility allows the reflective film to be optimized according to different application scenarios to meet specific needs. For example: If efficient reflection is required in a specific band (such as infrared or ultraviolet light), a can be accurately fitted based on the relationship between wavelength and refractive index. If certain specific spectral bands (such as visible light in sunlight) need to be reflected, the reflective performance can be customized by adjusting a and the number of film layers.
[0060] This specific embodiment also provides a reflective heat-insulating film including a reflective film, which includes: a wear-resistant layer, a reflective film, a functional layer, a UV-blocking pressure-sensitive adhesive layer, and a release film;
[0061] Among them, the functional layers are 0 to 5;
[0062] Among them, the functional layer includes a nano thermal insulation layer and a base film.
[0063] It is understood that the interference principle of the overlapping layers of resins involves the thin film interference phenomenon of light. Thin film interference is caused by the superposition of light waves after reflection and transmission at the interface of two or more different media. The overlapping of resin layer A and resin layer B forms a multilayer structure. The different layers of resin have different refractive indices and thicknesses. These differences will cause light waves to reflect and transmit at these interfaces, achieving complete reflection of all wavelengths of light (i.e., white light reflection).
[0064] In order to achieve complete reflection of all wavelengths of light, it is necessary for all wavelengths of light to meet the conditions of enhanced interference in the resin overlapping layers. This usually requires precise adjustment of the thickness and refractive index of each layer of resin so that for each wavelength, the light in this multilayer structure forms enhanced interference after coherent superposition of reflections. This specific implementation method can make all incident light waves meet the same coherence conditions when reflected on the interface of the multilayer structure by precisely designing the thickness of the resin A and resin B layers, thereby achieving reflection of all wavelengths of light. The relative average reflectivity of the wavelength of 400 to 700nm is more than 70%, and the reflectivity of the regular reflection component is more than 10% of the relative average reflectivity of the wavelength of 400 to 700nm.
[0065] In some preferred embodiments, the base film is a transparent or opaque polyester film, a polyurethane film, a polycarbonate film, or a laminated reflective film.
[0066] In some preferred embodiments, the total thickness of the reflective thermal insulation film is 53-556 μm.
[0067] In some preferred embodiments, the thickness of the laminated reflective film is 12-188 μm.
[0068] In some preferred embodiments, the thickness of the nano heat insulation layer is 3-30 μm.
[0069] In some preferred embodiments, the thickness of the UV blocking pressure-sensitive adhesive layer is 3-30 μm.
[0070] In some preferred embodiments, the thickness of the release film is 16-100 μm.
[0071] In some preferred embodiments, the wear-resistant layer has a thickness of 0.5-1 μm.
[0072] In some preferred embodiments, the thickness of the UV blocking pressure-sensitive adhesive layer is 3-50 μm.
[0073] In some preferred embodiments, the resin A layer is provided with protrusions, which are arranged in a dot matrix.
[0074] In this specific embodiment, the raised portions are arranged in a dot matrix, which introduces an additional optical path difference when light is incident, causing the incident light to diffract, causing light waves in different directions to interfere with each other, and improving the total reflectivity of light.
[0075] In some preferred embodiments, the height of the protrusion is 2-5 nm, and the bottom area of the protrusion is 4-8 nm. 2 .
[0076] It can be understood that the local thickness is changed by the raised portion, thereby changing the optical path difference in these local areas. The above-mentioned height and bottom area settings can achieve interference enhancement of light of specific wavelengths, such as infrared wavelengths, in these areas, thereby improving the reflectivity of infrared light.
[0077] In some preferred embodiments, the nano thermal insulation layer comprises the following components: an adhesive, a curing agent, a thermal insulation material, a solvent and a UV blocker;
[0078] Wherein, the adhesive is acrylic adhesive or polyurethane adhesive;
[0079] The curing agent is melamine or isocyanate;
[0080] The solvent is ethyl acetate, toluene or ketone;
[0081] The UV blocker can be benzotriazole, benzophenone or triazine.
[0082] The present embodiment provides a method for preparing a reflective thermal insulation film, comprising the following steps:
[0083] On one surface of the laminated reflective film, a mixed material for forming a wear-resistant layer is coated, and the wear-resistant layer is obtained after drying at a temperature of 70 to 130° C. and curing with ultraviolet light;
[0084] The mixed material of the UV-blocking pressure-sensitive adhesive layer is coated on the other surface of the laminated reflective film, and the mixed material is placed at a temperature of 90 to 150° C. for 40 to 120 seconds and then cured to obtain the UV-blocking pressure-sensitive adhesive layer;
[0085] Compounding the surface of the base film of the functional layer on the side of the UV blocking pressure-sensitive adhesive layer away from the laminated reflective film;
[0086] A release film is compounded on the surface of the nano heat-insulating layer of the functional layer to obtain a reflective heat-insulating film in which each layer is compounded into one.
[0087] Example 1
[0088] like Figure 1 As shown, this embodiment provides a reflective thermal insulation film, which includes: a wear-resistant layer 1, a laminated reflective film 2-1, a nano thermal insulation layer 3, a base film 2-2, a UV blocking pressure-sensitive adhesive layer 4 and a release film 5.
[0089] The thickness of the wear-resistant layer 1 is 0.5 μm, and the preparation method of the mixed material is as follows:
[0090] The scratch-resistant agent and solvent ethyl acetate were prepared in a mass ratio of 1:1.05, and the two were mixed evenly to obtain a mixed material for forming the wear-resistant layer 1, which was stored for later use. The mixed material had an appearance of a colorless transparent liquid and a solid content of 46wt%.
[0091] The thickness of the laminated reflective film 2 - 1 is 23 μm, and the material is a transparent polyester film.
[0092] The thickness of the nano heat-insulating layer 3 is 5 μm. The preparation method of the mixed material is as follows, calculated by mass percentage:
[0093] 6.23% of nano tungsten oxide was added to toluene, and the mixture was stirred for 30 minutes. 56.68% of acrylate adhesive was added, and the mixture was stirred for 25 minutes. 0.85% of curing agent was added, and the mixture was stirred for 5 to 15 minutes. The viscosity was measured to be 150 centipoise to obtain a mixed material.
[0094] The thickness of the base film 2 - 2 is 50 μm, and the material is a transparent polyester film.
[0095] The thickness of the UV-blocking pressure-sensitive adhesive layer 4 is 10 μm, and the preparation method of the mixed material is as follows:
[0096] Prepare the components in a mass ratio of acrylate adhesive: curing agent: toluene of 30:1.5:20. At an ambient temperature of 20°C, mix toluene and acrylate adhesive and stir for 20 minutes. Then add the curing agent and stir for another 10 minutes. The viscosity is measured by a rotational viscometer and is 120 centipoise.
[0097] Resin A is polyethylene terephthalate; Resin B is naphthenic acid copolyester;
[0098] The refractive index of the resin A layer is 1.655, and the refractive index of the resin B layer is 1.68.
[0099] Based on the above materials, this embodiment provides a method for preparing a reflective thermal insulation film, comprising the following steps:
[0100] On one surface of the laminated reflective film, a mixed material for forming a wear-resistant layer is coated, and the wear-resistant layer is obtained after drying at a temperature of 70 to 130° C. and curing with ultraviolet light;
[0101] The mixed material of the UV-blocking pressure-sensitive adhesive layer is coated on the other surface of the laminated reflective film, and the mixed material is placed at a temperature of 150° C. for 120 seconds and then cured to obtain the UV-blocking pressure-sensitive adhesive layer;
[0102] Compounding the surface of the base film of the functional layer on the side of the UV blocking pressure-sensitive adhesive layer away from the laminated reflective film;
[0103] A release film is compounded on the surface of the nano heat-insulating adhesive layer of the functional layer to obtain a reflective heat-insulating film with each layer compounded into one.
[0104] like Figure 2 As shown, in this embodiment, the resin overlapping layer is formed by overlapping and laying out a resin A layer 6 and a resin B layer 7, wherein the thickness of the resin A layer 6 is 100nm, and the thickness of the resin B layer 7, calculated according to the formula provided by the present invention, is 120nm.
[0105] Example 2
[0106] like Figure 1 As shown, this embodiment provides a reflective thermal insulation film, which includes: a wear-resistant layer 1, a laminated reflective film 2-1, a nano thermal insulation layer 3, a base film 2-2, a UV blocking pressure-sensitive adhesive layer 4 and a release film 5.
[0107] The thickness of the wear-resistant layer 1 is 0.8 μm, and the preparation method of the mixed material is as follows:
[0108] The scratch-resistant agent and solvent ethyl acetate were prepared in a mass ratio of 1:1.05, and the two were mixed evenly to obtain a mixed material for forming the wear-resistant layer 1, which was stored for later use. The mixed material had an appearance of a colorless transparent liquid and a solid content of 50wt%.
[0109] The thickness of the laminated reflective film 2 - 1 is 23 μm, and the material is a transparent polyester film.
[0110] The thickness of the nano heat-insulating layer 3 is 15 μm. The preparation method of the mixed material is as follows, calculated by mass percentage:
[0111] 6.23% of nano tungsten oxide was added to toluene, and the mixture was stirred for 30 minutes. 56.68% of acrylate adhesive was added, and the mixture was stirred for 25 minutes. 0.85% of curing agent was added, and the mixture was stirred for 5 to 15 minutes. The viscosity was measured to be 150 centipoise to obtain a mixed material.
[0112] The thickness of the base film 2 - 2 is 50 μm, and the material is a transparent polyester film.
[0113] Resin A is polyethylene terephthalate; Resin B is naphthenic acid copolyester;
[0114] The refractive index of the resin A layer is 1.655, and the refractive index of the resin B layer is 1.68.
[0115] The thickness of the UV-blocking pressure-sensitive adhesive layer 4 is 15 μm, and the preparation method of the mixed material is as follows:
[0116] Prepare the components in a mass ratio of acrylate adhesive: curing agent: toluene of 30:1.5:20. At an ambient temperature of 20°C, mix toluene and acrylate adhesive and stir for 20 minutes. Then add the curing agent and stir for another 10 minutes. The viscosity is measured by a rotational viscometer to be 200 centipoise.
[0117] Based on the above materials, this embodiment provides a method for preparing a reflective thermal insulation film, comprising the following steps:
[0118] On one surface of the laminated reflective film, a mixed material for forming a wear-resistant layer is coated, and the wear-resistant layer is obtained after drying at a temperature of 70 to 130° C. and curing with ultraviolet light;
[0119] The mixed material of the UV-blocking pressure-sensitive adhesive layer is coated on the other surface of the laminated reflective film, and the mixed material is placed at a temperature of 150° C. for 120 seconds and then cured to obtain the UV-blocking pressure-sensitive adhesive layer;
[0120] Compounding the surface of the base film of the functional layer on the side of the UV blocking pressure-sensitive adhesive layer away from the laminated reflective film;
[0121] A release film is compounded on the surface of the nano heat-insulating layer of the functional layer to obtain a reflective heat-insulating film in which each layer is compounded into one.
[0122] like Figure 3As shown, in this embodiment, the resin overlapping layer is formed by overlapping and laying out a resin A layer 6 and a resin B layer 7, wherein the thickness of the resin A layer 6 is 100nm, and the thickness of the resin B layer 7, calculated according to the formula provided by the present invention, is 110nm.
[0123] Example 3
[0124] like Figure 1 As shown, this embodiment provides a reflective thermal insulation film, which includes: a wear-resistant layer 1, a laminated reflective film 2-1, a nano thermal insulation layer 3, a base film 2-2, a UV blocking pressure-sensitive adhesive layer 4 and a release film 5.
[0125] The thickness of the wear-resistant layer 1 is 1 μm, and the preparation method of the mixed material is as follows:
[0126] The scratch-resistant agent and solvent ethyl acetate were prepared in a mass ratio of 1:1.05, and the two were mixed evenly to obtain a mixed material for forming the wear-resistant layer 1, which was stored for later use. The mixed material had an appearance of a colorless transparent liquid and a solid content of 46wt%.
[0127] The thickness of the laminated reflective film 2 - 1 is 23 μm, and the material is a transparent polyester film.
[0128] The thickness of the nano heat-insulating layer 3 is 20 μm. The preparation method of the mixed material is as follows, calculated by mass percentage:
[0129] 6.23% of nano tungsten oxide was added to toluene, and the mixture was stirred for 30 minutes. 56.68% of acrylate adhesive was added, and the mixture was stirred for 15 minutes. 0.85% of curing agent was added, and the mixture was stirred for 15 minutes. The viscosity was measured to be 150 centipoise to obtain a mixed material.
[0130] The thickness of the base film 2 - 2 is 50 μm, and the material is a transparent polyester film.
[0131] Resin A is polyethylene terephthalate; Resin B is naphthenic acid copolyester;
[0132] The refractive index of the resin A layer is 1.655, and the refractive index of the resin B layer is 1.68.
[0133] The thickness of the UV-blocking pressure-sensitive adhesive layer 4 is 15 μm, and the preparation method of the mixed material is as follows:
[0134] Prepare the components in a mass ratio of acrylate adhesive: curing agent: toluene of 30:1.5:20. At an ambient temperature of 20°C, first mix toluene and acrylate adhesive and stir for 10 minutes, then add curing agent and stir for another 10 minutes. The viscosity is measured by a rotational viscometer and is 120 centipoise.
[0135] Based on the above materials, this embodiment provides a method for preparing a reflective thermal insulation film, comprising the following steps:
[0136] On one surface of the laminated reflective film, a mixed material for forming a wear-resistant layer is coated, and the wear-resistant layer is obtained after drying at a temperature of 130° C. and curing with ultraviolet light;
[0137] The mixed material of the UV-blocking pressure-sensitive adhesive layer is coated on the other surface of the laminated reflective film, and the mixed material is placed at a temperature of 150° C. for 120 seconds and then cured to obtain the UV-blocking pressure-sensitive adhesive layer;
[0138] Compounding the surface of the base film of the functional layer on the side of the UV blocking pressure-sensitive adhesive layer away from the laminated reflective film;
[0139] A release film is compounded on the surface of the nano heat-insulating layer of the functional layer to obtain a reflective heat-insulating film in which each layer is compounded into one.
[0140] like Figure 4 and Figure 5 As shown, in this embodiment, the resin overlapping layer is formed by overlapping and laying out a resin A layer 6 and a resin B layer 7, wherein the thickness of the resin A layer 6 is 100nm, and the thickness of the resin B layer 7, calculated according to the formula provided by the present invention, is 105nm.
[0141] The resin A layer 6 is provided with a height of 2nm and a bottom area of 4nm. 2 The raised portions 61 are arranged in a dot matrix.
[0142] Performance Testing
[0143] Testing instrument: UV-visible near-infrared spectrophotometer
[0144] Test method: The instrument tests the reflection spectrum between 250nm-2500nm. The wavelength range of infrared reflection, reflectivity value and heat insulation barrier can be observed on the spectrum. Through the test monitoring of the full-band spectrophotometer, the wavelength of the infrared reflection film reflection band in the spectrum is observed. The spectrum of reflective films of different thicknesses shows different reflection wavelength ranges. The more infrared rays in sunlight it reflects, the more discomfort caused by radiant heat can be reduced by cutting off near infrared rays.
[0145] The above description is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been shown as a preferred embodiment, it is not intended to limit the present invention.
[0146] The present invention is defined, and any technician familiar with the profession can use the technical contents disclosed above to make some changes or modify them into equivalent embodiments with equivalent changes without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A laminated reflective film, It is characterized in that The laminated reflective film is a resin laminated layer formed by overlapping different resins; The resin overlapping layer includes a resin A layer and a resin B layer, The number of layers of the resin overlapped layer is 100 to 300; According to the adjustment of the thickness of the resin A layer and the thickness of the resin B layer, an interference reaction is generated to reflect light of different wavelengths in sunlight; The thickness of the resin A layer and the thickness of the resin B layer are determined by the following formula: Among them, h 1 and h 2 are the thickness of resin A layer and the thickness of resin B layer, respectively, in nm; γ 1 and γ 2 are the refractive indices of resin A layer and resin B layer respectively; a is the adjustment coefficient, the unit is 1; The thickness of the laminated reflective film is 10 to 200 μm.
2. A laminated reflective film according to claim 1, It is characterized in that The thickness of the resin A layer is 90-100 nm.
3. A laminated reflective film according to claim 1, It is characterized in that The a is determined according to the reflected infrared wavelength; The resin A contains polyethylene terephthalate or polyethylene naphthalate; the resin B is naphthenic acid copolymer polyester; The refractive index of the resin A layer is 1.655 to 1.70, and the refractive index of the resin B layer is 1.68 to 1.
72.
4. A reflective heat-insulating film comprising the laminated reflective film according to any one of claims 1 to 3, It is characterized in that The reflective heat-insulating film comprises, in sequence: a wear-resistant layer, a laminated reflective film, a functional layer, a UV-blocking pressure-sensitive adhesive layer and a release film; Wherein, the functional layer is 0 to 5 layers; Wherein, the functional layer includes a nano thermal insulation layer and a base film.
5. The reflective thermal insulation film according to claim 4, It is characterized in that The base film is a transparent polyester film or a laminated reflective film.
6. The reflective thermal insulation film according to claim 4, It is characterized in that The total thickness of the reflective thermal insulation film is 53-556 μm.
7. The reflective thermal insulation film according to claim 4, It is characterized in that The thickness of the laminated reflective film is 12 to 188 μm.
8. The reflective thermal insulation film according to claim 4, It is characterized in that The thickness of the nano heat insulation layer is 3-30 μm.
9. The reflective thermal insulation film according to claim 5, It is characterized in that The nano heat-insulating layer comprises the following components: an adhesive, a curing agent, a heat-insulating material, a solvent and an ultraviolet blocking agent.
10. A method for preparing a reflective thermal insulation film according to any one of claims 5 to 9, It is characterized in that The steps include: On one surface of the laminated reflective film, a mixed material for forming a wear-resistant layer is coated, and the wear-resistant layer is obtained after drying at a temperature of 70 to 130° C. and curing with ultraviolet light; The mixed material of the UV-blocking pressure-sensitive adhesive layer is coated on the other surface of the laminated reflective film, and the mixed material is placed at a temperature of 90 to 150° C. for 40 to 120 seconds and then cured to obtain the UV-blocking pressure-sensitive adhesive layer; Compounding the surface of the base film of the functional layer on the side of the UV blocking pressure-sensitive adhesive layer away from the laminated reflective film; A release film is compounded on the surface of the nano heat-insulating layer of the functional layer to obtain a reflective heat-insulating film in which each layer is compounded into one.