Pressure-resistant high-Tg epoxy adhesive and preparation method thereof
By adding thermoplastic resin to the epoxy resin to form a semi-interpenetrating network polymer, the problem of both compression strength and glass transition temperature after toughening modification of epoxy adhesive is solved, and high compression strength and high Tg's epoxy adhesive is suitable for areas with high impact resistance.
Patent Information
- Application Number
- CN202411178520.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
After toughening modification, existing epoxy adhesives are difficult to achieve high compression strength and high glass transition temperature at the same time, limiting their application in areas with high impact resistance requirements.
Thermoplastic resin is added to the continuous phase epoxy resin to form a semi-interpenetrating network polymer. The reaction between the phenoxy resin and the epoxy resin can improve the compressive strength and maintain a high glass transition temperature.
It significantly improves the compressive strength and shear strength of epoxy adhesives, while maintaining high glass transition temperature, and is suitable for electronic products and automobiles.
Smart Images

Figure BDA0005011426590000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy adhesives, in particular to a compression-resistant, high-Tg epoxy adhesive and a preparation method thereof. Background Art
[0002] Epoxy resin adhesive is a widely used type of adhesive in synthetic adhesive products, mainly composed of epoxy resin and curing agent. It began to be formally industrialized in the United States in 1947. Due to its excellent properties, such as good bonding performance, excellent mechanical properties, small curing shrinkage, good medium and heat resistance, and good chemical stability, it has quickly developed in the application of industry and other various bonding and potting fields.
[0003] Although epoxy adhesive has a wide range of uses, it also has major defects. For example, if it is not toughened and modified first, the cured epoxy adhesive will have poor crack resistance, hard and brittle texture, and low impact strength. These defects limit the application of epoxy adhesive in some electronic products and automotive products and other fields with high impact resistance requirements, so it is necessary to toughen and modify it to broaden its application areas and improve its use value.
[0004] At present, there are five main ways to strengthen and toughen epoxy adhesives:
[0005] (1) Use rubber elastomers, thermotropic liquid crystals and other second phase toughening modification. Rubber toughening is to disperse rubber particles in the cured epoxy resin matrix. This toughening mainly strengthens the cured product. The rubber toughening agent needs to meet several conditions:
[0006] ① The size of rubber particles should be appropriate (0.1-0.2μm); ② The rubber particles should have an appropriate elastic modulus; ③ The rubber particles should be able to bond well with the matrix resin. Due to these special requirements, this toughening method is technically complex and difficult to achieve industrialization.
[0007] (2) Use thermoplastics to continuously penetrate the epoxy resin network to form a semi-interpenetrating network polymer toughening modification. This toughening method is more commonly used in the field of thermoplastic resins, but is not suitable for toughening modification of thermosetting resins, and its application range is limited.
[0008] (3) Toughening by changing the chemical structure of the cross-linked network (such as introducing a "flexible segment" into the cross-linked network) to increase the activity of the cross-linked network. For the cross-linked network of epoxy resin matrix with high cross-linking density and high brittleness, the effect of toughening with rubber elastomers is not very obvious, and the glass transition temperature and modulus of the toughened material are significantly reduced. At this time, it is necessary to add some "flexible segments" with strong activity but good heat resistance to the above system to increase the activity of network molecules. Therefore, this method is only applicable to epoxy resin with high cross-linking density and high brittleness.
[0009] (4) Toughening is achieved by controlling the inhomogeneity of the molecular cross-linking state to form a non-uniform structure that is conducive to plastic deformation. This method uses in-situ toughening technology and is achieved through a two-stage reaction. Its toughening mechanism is due to the inhomogeneity of the cross-linking network of the epoxy resin cured product, thereby forming a microscopic non-uniform continuous structure to achieve toughening of the EP glue. However, how to better control the structural morphology of the final cured product from the perspective of the chemical reaction mechanism so that it is conducive to improving toughness is an important problem that has not yet been solved by this method.
[0010] (5) Use inorganic fillers for toughening. The ultrafine particles and fibers in the inorganic fillers are combined with the matrix through bonding forces such as hydrogen bonds, so that the EP adhesive composite material concentrates stress to produce micro cracks and absorb a certain amount of deformation work, preventing the material from cracking malignantly and restraining the crack propagation, thereby playing a role in toughening and modification.
[0011] However, currently, none of the above methods can produce a single-component epoxy structural adhesive with high compressive strength, high Tg, and high shear strength. Therefore, how to obtain high compressive strength without lowering the glass transition temperature has become a research direction in the industry. Summary of the invention
[0012] The object of the present invention is to provide a compression-resistant, high Tg epoxy adhesive and a preparation method thereof, by adding a thermoplastic resin to a continuous phase epoxy resin to form a semi-interpenetrating network polymer to achieve toughening modification. The problem that general toughening agents, after being physically mixed into the epoxy resin curing system, will cause the crosslinking density of the epoxy resin to decrease, thereby causing the glass transition temperature to decrease, is solved. The thermoplastic resin used in the present invention is a phenoxy resin, and its active group participates in the reaction during the epoxy resin curing process, thereby "grafting" the phenoxy resin to the epoxy resin system, effectively improving the compression strength of the epoxy structural adhesive, which can meet the application of electronic products, automotive products and other fields with high impact requirements.
[0013] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0014] A compression-resistant, high Tg epoxy adhesive comprises a phenoxy resin solution and an epoxy polymer. The phenoxy resin solution is obtained by dissolving a phenoxy resin in a diluent, and the solid content thereof is 20%. The epoxy polymer comprises the following components in parts by weight: 100 parts of bisphenol A epoxy resin, 45-65 parts of a curing agent, 10-30 parts of calcium carbonate, and 1-5 parts of a silane coupling agent. The weight ratio of the phenoxy resin solution to the epoxy polymer is (0.1-0.6):1.
[0015] Further, the phenoxy resin is selected from at least one of a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a bisphenol acetophenone skeleton, a phenolic skeleton, a biphenyl skeleton, a fluorene skeleton, a dicyclopentadiene skeleton, a norbornene skeleton, a naphthalene skeleton, an anthracene skeleton, an adamantane skeleton, a terpene skeleton and a trimethylcyclohexane skeleton; for example, PKHH with a bisphenol A skeleton is preferred.
[0016] Furthermore, the diluent is at least one of phenyl glycidyl ether, o-benzyl glycidyl ether, butyl glycidyl ether, and octyl glycidyl ether; for example, preferred o-benzyl glycidyl ether XY691 and phenyl glycidyl ether XY690A.
[0017] Furthermore, the bisphenol A epoxy resin is at least one of E51 and E44; for example, the preferred bisphenol A epoxy resin NEL-128 with an epoxy value of 0.48-0.54 is E-51.
[0018] Furthermore, the curing agent is at least one of methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, dichloromaleic anhydride, tung oil anhydride, and glutaric anhydride; for example, methylhexahydrophthalic anhydride is preferred.
[0019] Furthermore, the calcium carbonate is nano calcium carbonate; calcium carbonate in epoxy adhesive not only improves the strength and hardness of the adhesive, but also has the function of reducing curing shrinkage and adjusting viscosity, while reducing production costs; for example, the preferred calcium carbonate is P270 with an average particle size of 80±30nm from Warner New Materials.
[0020] Furthermore, the silane coupling agent is 3-glycidyloxypropyltrimethoxysilane; for example, a preferred silane coupling agent may be KH560.
[0021] The weight ratio of the phenoxy resin solution to the epoxy polymer is limited to (0.1-0.6): 1; the amount of the added phenoxy resin solution is crucial to the compressive strength, Tg, and shear strength of the epoxy adhesive. Specifically, if a high content of phenoxy resin is added, a high content of active diluent will also be introduced, resulting in a decrease in the Tg and shear strength of the epoxy adhesive; if the amount of the added phenoxy resin solution is too small, it will not have the effect of improving the compressive strength.
[0022] Furthermore, the mass ratio of the phenoxy resin solution to the epoxy polymer is preferably (0.2-0.4):1, and may also be a ratio consisting of any point value within the range.
[0023] A method for preparing a compression-resistant, high Tg epoxy adhesive comprises the following steps:
[0024] S1: Preparation of phenoxy resin solution
[0025] The temperature of the heating table is controlled at 70-90°C, the diluent is weighed in a beaker, the phenoxy resin is added, and a magnetic bar is added to stir until the phenoxy resin particles completely disappear and the solution becomes transparent, thereby obtaining a phenoxy resin solution;
[0026] S2: Preparation of epoxy polymers
[0027] The following raw materials in parts by weight are mixed to obtain an epoxy polymer;
[0028] 100 parts of bisphenol A epoxy resin,
[0029] 45-65 parts of curing agent,
[0030] 10-30 parts calcium carbonate,
[0031] 1-5 parts of silane coupling agent;
[0032] S3: Preparation of epoxy structural adhesive
[0033] The phenoxy resin solution in step S1 is added to the epoxy polymer in step S2 and stirred for 3-5 hours to obtain an epoxy structural adhesive.
[0034] Furthermore, in step S2, bisphenol A epoxy resin and curing agent are first mixed, then a silane coupling agent is added, and then calcium carbonate powder is added; the bisphenol A epoxy resin and the curing agent undergo an addition reaction to generate an ester bond.
[0035] Furthermore, in step S3, the raw materials are added while stirring.
[0036] A compression-resistant, high Tg epoxy adhesive. According to tests, the annular performance compression strength of the epoxy adhesive is above 320N and the Tg is above 180°C.
[0037] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0038] (1) The present invention prepares epoxy adhesive by adding phenoxy resin solution to epoxy polymer, thereby improving the compression resistance of epoxy adhesive. The annular performance compression strength can reach 320N, which is 50% higher than that of ordinary epoxy structural adhesive.
[0039] (2) Select a suitable diluent to dissolve the phenoxy resin into a liquid to be added to the epoxy polymer; at the same time, the diluent contains epoxy groups, which can actively participate in the curing reaction of the epoxy resin, thereby forming a stable and strong network structure with the main components of the epoxy adhesive, enhancing the overall strength of the adhesive and significantly improving its shear strength.
[0040] (3) The phenoxy resin in the present invention can be efficiently dissolved in epoxy resin at a suitable temperature because it contains hydroxyl groups and has a molecular structure similar to that of epoxy resin. Moreover, the phenolic hydroxyl groups in its molecules can easily form a stable hydrogen bond network structure with epoxy resin, thereby optimizing the viscosity and viscoelastic properties, achieving the best hydrogen bond network morphology, and hindering the reduction of the glass transition temperature of the epoxy adhesive; therefore, after adding phenoxy resin, the compression resistance of the epoxy adhesive can be improved while affecting its glass transition temperature as little as possible. DETAILED DESCRIPTION
[0041] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] First, the raw materials used in this application are shown in the following table:
[0043]
[0044] Example and comparative example settings:
[0045] Example 1
[0046] A compression-resistant, high Tg epoxy adhesive is prepared by the following method, comprising the following steps:
[0047] S1: Preparation of phenoxy resin solution
[0048] The heating table is heated to 80°C, 80 parts of diluent XY691 and 20 parts of phenoxy resin PKHH are weighed and added into a beaker, and a magnetic bar is added to stir until the particles completely disappear and the solution becomes transparent, thereby obtaining a phenoxy resin solution with a solid content of 20%;
[0049] S2: Preparation of epoxy polymers
[0050] First, 100 parts of bisphenol A epoxy resin and 45 parts of curing agent are uniformly mixed, then 1 part of silane coupling agent is added, and then 30 parts of nano calcium carbonate powder are added and mixed to obtain epoxy polymer;
[0051] S3: Preparation of epoxy structural adhesive
[0052] 10 parts of the phenoxy resin solution in step S1 were added to 100 parts of the epoxy polymer in step S2, and stirred for 1.5 hours to obtain an epoxy structural adhesive.
[0053] Example 2
[0054] A compression-resistant, high Tg epoxy adhesive is prepared by the following method, comprising the following steps:
[0055] S1: Preparation of phenoxy resin solution
[0056] The heating table is heated to 80°C, 80 parts of diluent XY690A and 20 parts of phenoxy resin PKHH are weighed and added into a beaker, and a magnetic bar is added to stir until the particles completely disappear and the solution becomes transparent, thereby obtaining a phenoxy resin solution with a solid content of 20%;
[0057] S2: Preparation of epoxy polymers
[0058] First, 100 parts of bisphenol A epoxy resin and 50 parts of curing agent are uniformly mixed, then 3 parts of silane coupling agent are added, and then 25 parts of nano calcium carbonate powder are added and mixed to obtain epoxy polymer;
[0059] S3: Preparation of epoxy structural adhesive
[0060] 20 parts of the phenoxy resin solution in step S1 were added to 100 parts of the epoxy polymer in step S2, and stirred for 1.5 hours to obtain an epoxy structural adhesive.
[0061] Example 3
[0062] A compression-resistant, high Tg epoxy adhesive is prepared by the following method, comprising the following steps:
[0063] S1: Preparation of phenoxy resin solution
[0064] The heating table is heated to 80°C, 80 parts of diluent XY691 and 20 parts of phenoxy resin PKHH are weighed and added into a beaker, and a magnetic bar is added to stir until the particles completely disappear and the solution becomes transparent, thereby obtaining a phenoxy resin solution with a solid content of 20%;
[0065] S2: Preparation of epoxy polymers
[0066] First, 100 parts of bisphenol A epoxy resin and 55 parts of curing agent are uniformly mixed, then 5 parts of silane coupling agent are added, and then 20 parts of nano calcium carbonate powder are added and mixed to obtain epoxy polymer;
[0067] S3: Preparation of epoxy structural adhesive
[0068] 40 parts of the phenoxy resin solution in step S1 were added to 100 parts of the epoxy polymer in step S2, and stirred for 1.5 hours to obtain an epoxy structural adhesive.
[0069] Example 4
[0070] A compression-resistant, high Tg epoxy adhesive is prepared by the following method, comprising the following steps:
[0071] S1: Preparation of phenoxy resin solution
[0072] The heating table is heated to 80°C, 80 parts of diluent XY691 and 20 parts of phenoxy resin PKHH are weighed and added into a beaker, and a magnetic bar is added to stir until the particles completely disappear and the solution becomes transparent, thereby obtaining a phenoxy resin solution with a solid content of 20%;
[0073] S2: Preparation of epoxy polymers
[0074] First, 100 parts of bisphenol A epoxy resin and 65 parts of curing agent are uniformly mixed, then 5 parts of silane coupling agent are added, and then 10 parts of nano calcium carbonate powder are added and mixed to obtain epoxy polymer;
[0075] S3: Preparation of epoxy structural adhesive
[0076] 60 parts of the phenoxy resin solution in step S1 were added to 100 parts of the epoxy polymer in step S2, and stirred for 1.5 hours to obtain an epoxy structural adhesive.
[0077] Comparative Example 1
[0078] Compared with Example 1, no phenoxy resin solution is added to the epoxy structural adhesive. The preparation method only includes the preparation of epoxy polymer, firstly, 100 parts of bisphenol A epoxy resin and 45 parts of curing agent are evenly mixed, then 1 part of silane coupling agent is added, and then 30 parts of nano calcium carbonate powder are added and mixed to obtain epoxy polymer, i.e. epoxy structural adhesive.
[0079] Comparative Example 2
[0080] Compared with Example 1, the phenoxy resin solution is not added to the epoxy structural adhesive, but a liquid CTBN toughening agent is added to the epoxy polymer. The preparation method is as follows:
[0081] S1: Preparation of epoxy polymers
[0082] First, 100 parts of bisphenol A epoxy resin and 45 parts of curing agent are uniformly mixed, then 1 part of silane coupling agent is added, and then 30 parts of nano calcium carbonate powder are added and mixed to obtain epoxy polymer;
[0083] S2: Add 2 parts of CTBN toughening agent to 100 parts of the epoxy polymer in step S1, and stir for 1.5 hours to obtain epoxy structural adhesive.
[0084] Comparative Example 3
[0085] S1: Preparation of phenoxy resin solution
[0086] The heating table is heated to 80°C, 80 parts of diluent XY691 and 20 parts of phenoxy resin PKHH are weighed and added into a beaker, and a magnetic bar is added to stir until the particles completely disappear and the solution becomes transparent, thereby obtaining a phenoxy resin solution with a solid content of 20%;
[0087] S2: Preparation of epoxy polymers
[0088] First, 100 parts of bisphenol A epoxy resin and 55 parts of curing agent are uniformly mixed, then 5 parts of silane coupling agent are added, and then 20 parts of nano calcium carbonate powder are added and mixed to obtain epoxy polymer;
[0089] S3: Preparation of epoxy structural adhesive
[0090] 5 parts of the phenoxy resin solution in step S1 were added to 100 parts of the epoxy polymer in step S2, and stirred for 1.5 hours to obtain an epoxy structural adhesive.
[0091] Comparative Example 4
[0092] S1: Preparation of phenoxy resin solution
[0093] The heating table is heated to 80°C, 80 parts of diluent XY691 and 20 parts of phenoxy resin PKHH are weighed and added into a beaker, and a magnetic bar is added to stir until the particles completely disappear and the solution becomes transparent, thereby obtaining a phenoxy resin solution with a solid content of 20%;
[0094] S2: Preparation of epoxy polymers
[0095] First, 100 parts of bisphenol A epoxy resin and 55 parts of curing agent are uniformly mixed, then 5 parts of silane coupling agent are added, and then 20 parts of nano calcium carbonate powder are added and mixed to obtain epoxy polymer;
[0096] S3: Preparation of epoxy structural adhesive
[0097] 80 parts of the phenoxy resin solution in step S1 were added to 100 parts of the epoxy polymer in step S2, and stirred for 1.5 hours to obtain an epoxy structural adhesive.
[0098] test
[0099] The epoxy adhesives of Example 1N4 and Comparative Example 1N4 were tested for ring performance compression strength, glass transition temperature (Tg), and shear strength. The specific test methods are as follows:
[0100] (1) Ring performance compression strength: The epoxy adhesive is cured in the fixture according to the curing conditions to form a rubber ring with an inner diameter of 8 mm, an outer diameter of 14 mm, and a thickness of 3 mm. The force [N] required to break the ring is tested;
[0101] (2) Glass transition temperature: The glass transition temperature of the cured product was measured using the DSC temperature scanning mode [°C];
[0102] (3) Shear strength: SUS304 was selected as the bonding substrate, and the dynamic shear strength [MPa] of the epoxy adhesive cured product was tested according to the ASTM D1002 method.
[0103] The test results are shown in Table 1.
[0104] Table 1
[0105] Ring performance compression strength [N] Tg[℃] Shear strength[MPa] Example 1 250.2 190 21.9 Example 2 280.9 188 22.5 Example 3 320.9 185 23.8 Example 4 278.2 181 21.3 Comparative Example 1 210.2 192 21.5 Comparative Example 2 318.5 170 21.9 Comparative Example 3 225.8 190 23.2 Comparative Example 4 266.8 168 20.7
[0106] Conclusion: It can be seen from the data in the table that Examples 1-4 prepared by the technical solution of the present invention control the weight ratio of phenoxy resin solution to epoxy polymer to be (0.1-0.6):1, and add phenoxy resin solution to epoxy polymer, which can improve the compressive strength of the obtained epoxy structural adhesive without affecting the glass transition temperature, and make the shear strength above 21 MPa.
[0107] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A compression-resistant, high Tg epoxy adhesive, characterized in that: The invention comprises a phenoxy resin solution and an epoxy polymer. The phenoxy resin solution is obtained by dissolving a phenoxy resin in a diluent, and the solid content of the phenoxy resin solution is 20%. The epoxy polymer comprises the following components in parts by weight: 100 parts of bisphenol A epoxy resin, 45-65 parts of curing agent, 10-30 parts of calcium carbonate, 1-5 parts of silane coupling agent; the weight ratio of the phenoxy resin to the epoxy polymer is (0.1-0.6):
1.
2. The epoxy adhesive according to claim 1, characterized in that: The phenoxy resin is selected from at least one of a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a bisphenol acetophenone skeleton, a phenolic skeleton, a biphenyl skeleton, a fluorene skeleton, a dicyclopentadiene skeleton, a norbornene skeleton, a naphthalene skeleton, an anthracene skeleton, an adamantane skeleton, a terpene skeleton and a trimethylcyclohexane skeleton.
3. The epoxy adhesive according to claim 1, characterized in that: The diluent is at least one of phenyl glycidyl ether, o-benzyl glycidyl ether, butyl glycidyl ether and octyl glycidyl ether.
4. The epoxy adhesive according to claim 1, characterized in that: The bisphenol A epoxy resin is at least one of E51 and E44.
5. The epoxy adhesive according to claim 1, characterized in that: The curing agent is at least one of methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, dichloromaleic anhydride, tung oil anhydride and glutaric anhydride.
6. The epoxy adhesive according to claim 1, characterized in that: The calcium carbonate is nano calcium carbonate.
7. The epoxy adhesive according to claim 1, characterized in that: The silane coupling agent is 3-glycidyloxypropyltrimethoxysilane.
8. A method for preparing a compression-resistant, high Tg epoxy adhesive, comprising the following steps: S1: Preparation of phenoxy resin solution The temperature of the heating table is controlled at 70-90°C, the diluent is weighed in a beaker, phenoxy resin is added, and a magnetic bar is added to stir until the particles completely disappear and the solution becomes transparent, thereby obtaining a phenoxy resin solution; S2: Preparation of epoxy polymers Mixing 100 parts by weight of bisphenol A epoxy resin, 45-65 parts by weight of curing agent, 10-30 parts by weight of calcium carbonate, and 1-5 parts by weight of silane coupling agent to obtain an epoxy polymer; S3: Preparation of epoxy structural adhesive The phenoxy resin solution in step S1 is added to the epoxy polymer in step S2, and stirred for 3-5 hours to obtain an epoxy structural adhesive.
9. The method for preparing the epoxy adhesive according to claim 8, characterized in that: In the step s2, bisphenol A epoxy resin and curing agent are first mixed, then a silane coupling agent is added, and then calcium carbonate powder is added; In the step S3, the raw materials are added while stirring.
10. The epoxy adhesive according to any one of claims 1 to 7 or the epoxy adhesive prepared according to any one of claims 8 to 9, characterized in that: After testing, the Tg of the epoxy adhesive is above 180°C.