Thermosetting flexible encapsulating material as well as preparation method and application thereof

By using thermoset flexible adhesive wrapping materials, combined with specific components and preparation methods, the problems of large hardness of thermoset materials and poor adhesion of thermoplastic elastomers are solved, and high adhesion and high temperature resistance to metal materials are achieved, and flexible and anti-slip function covering effect.

CN119060671APending Publication Date: 2024-12-03SWANCOR ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411331397.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing thermosetting materials have a high hardness after curing, and cannot achieve anti-slip, shock absorption and soft touch coating effects on metal materials. Moreover, the adhesiveness and compatibility of thermoplastic elastomers to metal materials are poor, making it difficult to achieve effective coating. .

Method used

A thermoset flexible adhesive encapsulating material is adopted, including bisphenol A type epoxy resin, polyether modified epoxy resin, epoxy modified core-shell nanoparticle toughening agent, monofunctional aliphatic glycidyl ether cross-linking terminator, Components such as silane coupling agents, aliphatic polyamine curing agents, etc. form flexible encapsulated materials with high adhesion and high temperature resistance through specific preparation methods and process conditions.

Benefits of technology

It achieves high adhesion and high temperature resistance to metal materials, can be used for a long time under high temperature conditions, has functions such as flexibility and anti-slip, and is suitable for metal materials covering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060671A_ABST
    Figure CN119060671A_ABST
Patent Text Reader

Abstract

The invention provides a thermosetting flexible encapsulation material as well as a preparation method and application thereof, and belongs to the technical field of encapsulation. The epoxy resin composition comprises the following components: epoxy resin, a diluent, a flexible toughening agent, a cross-linking terminator, a coupling agent, a curing agent and a curing accelerator. The thermosetting flexible rubber coating material provided by the invention has extremely high adhesive strength and high temperature resistance on metal materials, and can be used for a long time under a high-temperature condition without the phenomena of melting, falling off and the like when being used for coating rubber on the metal materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a thermosetting flexible rubber coating material, a preparation method and application thereof, and belongs to the technical field of rubber coating. Background Art

[0002] Encapsulation, also known as overmolding, is the process of encapsulating soft rubber materials onto the surface of other materials to give the product functional properties such as soft touch, non-slip, wear resistance, shock absorption, elasticity, sealing, and waterproofness to meet the specific usage scenarios of the product.

[0003] In practical applications, commonly used encapsulation materials are mainly thermoplastic elastomers, such as TPE, PVC, POE and other materials, which are encapsulated on other materials by secondary injection molding. However, the products that can be encapsulated are limited. For example, plastic products such as PP / PE can be directly encapsulated, but the encapsulation effect on hard materials such as metal materials and FRP is poor and cannot be directly encapsulated.

[0004] This is because metal materials basically do not flow at high temperatures, and thermoplastic elastomer coating materials and metal materials cannot be connected by fusion welding. In addition, due to the poor compatibility of the two materials, the bonding force of the contact surface of the two materials is extremely low, and it is difficult for thermoplastic elastomers to effectively coat metal materials.

[0005] Currently, there is a method on the market to improve the adhesion of thermoplastic elastomers to metal materials by brushing adhesive on the surface of metal materials. This method is complex in process and difficult to operate, and is not suitable for mass production.

[0006] The molecular weight of thermoplastic elastomers ranges from tens of thousands to hundreds of thousands. They are solid particles at room temperature and need to be melted at high temperatures. Their fluidity is also poor at high temperatures, requiring high-temperature and high-pressure injection molding, which consumes a lot of energy. In addition, as products become more complex, product sizes vary greatly and requirements are complex, especially when there are many special-shaped parts to be coated. Thermoplastic elastomer coating materials have insufficient fluidity and are usually unable to achieve uniform coating.

[0007] Thermoplastic elastomers rely on van der Waals forces to form physical cross-linking points, and have no chemical cross-linking points. Therefore, they have poor wear resistance, corrosion resistance, and high temperature resistance.

[0008] Conventional thermosetting materials, although they have a chemically cross-linked structure, which greatly improves their wear resistance, corrosion resistance, and high temperature resistance compared to thermoplastic materials, are very hard after curing, and after being encapsulated, they cannot provide anti-slip, shock absorption, and soft touch effects.

[0009] Therefore, there is an urgent need for a thermosetting flexible encapsulating material in the art. Summary of the invention

[0010] The purpose of the present invention is to solve the problem that the thermosetting material in the prior art, although having a chemically cross-linked structure, has a high hardness after curing and cannot play the role of anti-slip, shock absorption, and soft touch after being encapsulated.

[0011] In order to achieve the purpose of solving the above problems, the technical solution adopted by the present invention is to provide a thermosetting flexible encapsulation material, a preparation method and application thereof

[0012] The first aspect of the present invention provides a thermosetting flexible encapsulation material, comprising the following components:

[0013]

[0014] Preferably, the epoxy resin comprises bisphenol A epoxy resin.

[0015] Preferably, the diluent comprises at least one of a polyol or a difunctional aliphatic glycidyl ether.

[0016] Preferably, the flexible toughening agent includes at least one of a polyether-modified epoxy resin and an epoxy-modified core-shell nanoparticle toughening agent.

[0017] Preferably, the cross-linking terminator comprises at least one of monofunctional aliphatic glycidyl ether and monofunctional aliphatic glycidyl ester.

[0018] Preferably, the coupling agent comprises a silane coupling agent.

[0019] Preferably, the curing agent includes at least one of aliphatic polyamine, polyetheramine or modified polyetheramine.

[0020] Further preferably, the modified polyetheramine has the structural formula:

[0021]

[0022] Wherein, m and n are natural numbers greater than 1; the modified polyetheramine composition has a wavelength of 1000 to 7500 cm in infrared spectrum analysis. -1 Characteristic peak.

[0023] Preferably, the curing accelerator comprises an amine accelerator.

[0024] The second aspect of the present invention provides a method for preparing the above-mentioned thermosetting flexible encapsulating material, comprising the following steps:

[0025] Step 1, putting epoxy resin, diluent and flexible toughening agent into a reaction kettle, heating and stirring, after the reaction is completed, returning the reaction kettle to room temperature, adding coupling agent and cross-linking terminator, stirring, and obtaining the main agent;

[0026] Step 2, accurately weigh the curing agent, add the diluent dropwise under heating conditions, cool after the reaction is completed, add the curing agent and curing accelerator, stop stirring after the reaction is completed, and obtain the auxiliary agent;

[0027] Step 3: Evenly mix the main agent obtained in step 1 and the auxiliary agent obtained in step 2 in a ratio of 100:20-30 to obtain a thermosetting flexible encapsulating material.

[0028] The third aspect of the present invention provides an application method of the above-mentioned thermosetting flexible encapsulating material, comprising the following steps: when encapsulating the metal material, the thermosetting flexible encapsulating material is added to the mold by infusion or the like, and then heated at 70°C for 10 minutes for curing, and then demolding can achieve the encapsulation of the metal material with the flexible epoxy resin.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The thermosetting flexible encapsulating material provided by the present invention has extremely high adhesion to metal materials and high temperature resistance. The encapsulating material can be used for a long time under high temperature conditions without melting, falling off, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the structural identification spectrum of modified polyetheramine and polyetheramine. DETAILED DESCRIPTION

[0032] In order to make the present invention more clearly understood, a preferred embodiment is described in detail with reference to the accompanying drawings as follows:

[0033] like Figure 1 As shown, the present invention provides a thermosetting flexible encapsulating material, a preparation method and application thereof.

[0034] The components and their corresponding mass percentages in the raw materials used in Examples 1-3 are shown in Table 1.

[0035] Table 1

[0036]

[0037]

[0038] Example 1

[0039] (1) putting bisphenol A epoxy resin, polyether modified epoxy resin, polyol, epoxy modified core-shell nanoparticle toughening agent, and monofunctional aliphatic glycidyl ether into a reactor, heating the reactor to 60° C., turning on the stirrer, stirring at a speed of 60 rpm for 60 minutes and then stopping, returning the reactor to room temperature, adding silane coupling agent, turning on the stirrer, stirring at a speed of 60 rpm for 10 minutes and then stopping to obtain the main agent;

[0040] (2) After accurately weighing the polyetheramine, add it to another reactor, heat the reactor to 80° C., turn on the stirrer, continue stirring at a speed of 60 rpm, and add 15 parts of aliphatic glycidyl ether by dropwise addition. After the addition is complete, stir for 120 minutes to obtain a modified polyetheramine. After cooling to 60° C., add aliphatic polyamine and amine accelerator to the reactor, continue stirring at a speed of 60 rpm for 30 minutes. After bisphenol A is completely dissolved, stop stirring, and return the reactor to room temperature to obtain the auxiliary agent.

[0041] (3) The main agent of step (1) and the auxiliary agent of step (2) are mixed evenly in a ratio of 100:25 to obtain the thermosetting flexible encapsulating material.

[0042] When encapsulating the metal material, the composition of step (3) is added into the mold by means of infusion or the like, and then heated at 70° C. for 10 minutes for curing, and then demolded to achieve encapsulation of the metal material with the flexible epoxy resin.

[0043] Example 2

[0044] Keeping other conditions unchanged, the components in the preparation raw materials and their corresponding mass percentages are shown in Table 1.

[0045] Example 3

[0046] Keeping other conditions unchanged, the components in the preparation raw materials and their corresponding mass percentages are shown in Table 1.

[0047] Comparative Example 1

[0048] Commercially available TPE encapsulated particles are used, and after the encapsulated particles are melted at 140° C., the metal material is encapsulated by an injection molding process, and after cooling, the encapsulated product is demoulded to obtain.

[0049] Comparative Example 2

[0050] Commercially available TPE encapsulated particles are used, and after the encapsulated particles are melted at 120° C., the metal material is encapsulated by an injection molding process, and the encapsulated product is demoulded after cooling.

[0051] Comparative Example 3

[0052] Conventional bisphenol A type thermosetting epoxy resin is used in a ratio of 100:15 with an amine curing agent, and the encapsulation is cured at 70℃*10min.

[0053] Performance testing experiment

[0054] Experimental samples: Examples 1-3 are numbered as experimental samples 1-3 in sequence; Comparative Examples 1-3 are numbered as control samples 1-3 in sequence. The results are shown in Table 2.

[0055] Judging Method:

[0056] The test samples were subjected to a roller peeling test according to GB / T 1457-2022 standard to test the adhesion of the lagging material to the metal material.

[0057] The test sample was placed at 100°C and baked for 8 hours, and the deformation of the metal surface coating material was observed to test the high temperature resistance of the coating material.

[0058] Table 2

[0059]

[0060]

[0061] It can be seen from the results of Example 1, Comparative Example 1, Comparative Example 2 and Table 2 that, compared with conventional thermoplastic elastomer encapsulation materials, the thermosetting flexible encapsulation material provided by the present invention has extremely high adhesion to metal materials and high temperature resistance. The encapsulation of metal materials can be used for a long time under high temperature conditions without melting, falling off, etc.

[0062] It can be seen from the results of Example 1, Comparative Examples 1-3 and Table 2 that, compared with conventional thermosetting materials, the thermosetting flexible encapsulating material provided by the present invention has extremely low hardness and excellent flexibility, and its hardness is comparable to that of thermoplastic encapsulating materials. Therefore, it can provide good elastic touch for metal materials and play a protective and anti-slip role.

[0063] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and equivalent changes made by using the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A thermosetting flexible encapsulation material, characterized in that: Includes the following components:

2. The thermosetting flexible lagging material according to claim 1, characterized in that: The epoxy resin includes bisphenol A type epoxy resin.

3. The thermosetting flexible lagging material according to claim 1, characterized in that: The diluent includes at least one of polyols or difunctional aliphatic glycidyl ethers.

4. The thermosetting flexible lagging material according to claim 1, characterized in that: The flexible toughening agent comprises at least one of a polyether modified epoxy resin and an epoxy modified core-shell nanoparticle toughening agent.

5. The thermosetting flexible lagging material according to claim 1, characterized in that: The cross-linking terminator includes at least one of monofunctional aliphatic glycidyl ether and monofunctional aliphatic glycidyl ester.

6. The thermosetting flexible lagging material according to claim 1, characterized in that: The curing agent includes at least one of aliphatic polyamine, polyetheramine or modified polyetheramine.

7. The thermosetting flexible lagging material according to claim 1, characterized in that: The modified polyetheramine structural formula is: Wherein, m and n are natural numbers greater than 1; the modified polyetheramine composition has a wavelength of 1000 to 7500 cm in infrared spectrum analysis. -1 Characteristic peak.

8. The thermosetting flexible lagging material according to claim 1, characterized in that: The curing accelerator includes an amine accelerator.

9. A method for preparing a thermosetting flexible encapsulating material as claimed in claim 1, characterized in that: The following steps are involved: Step 1, putting epoxy resin, diluent and flexible toughening agent into a reaction kettle, heating and stirring, after the reaction is completed, returning the reaction kettle to room temperature, adding coupling agent and cross-linking terminator, stirring, and obtaining the main agent; Step 2, accurately weigh the curing agent, add the diluent dropwise under heating conditions, cool after the reaction is completed, add the curing agent and curing accelerator, stop stirring after the reaction is completed, and obtain the auxiliary agent; Step 3: Evenly mix the main agent obtained in step 1 and the auxiliary agent obtained in step 2 in a ratio of 100:20-30 to obtain a thermosetting flexible encapsulating material.

10. An application method of the thermosetting flexible encapsulating material according to claim 1, characterized in that: The following steps are involved: When encapsulating metal materials, the thermosetting flexible encapsulating material is added into the mold by infusion or the like, and then heated at 70°C for 10 minutes for curing. After that, demolding can be performed to realize the encapsulation of the metal material by the flexible epoxy resin.