Method for preparing biochar through continuous pyrolysis of salix psammophila
The preparation of biochar by hydrothermal carbonization method has solved the problems of high temperature and high pressure and large gas emissions of existing pyrolysis methods, and achieved efficient preparation of hydrothermal carbon with high adsorption performance.
Patent Information
- Application Number
- CN202411180817.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
When the existing pyrolysis chemical conversion method is used to prepare biochar, the temperature and pressure are high, resulting in a large amount of CO2 and harmful gas emissions and low carbonization efficiency.
Using the hydrothermal carbonization method, the salis wood powder and water are mixed in a polytetrafluoroethylene lined hydrothermal reactor, heated to 230-290℃, kept for 24-48 hours, filtered and washed after cooling, and obtained hydrothermal carbon .
It reduces the preparation temperature and harmful gas emissions, improves the adsorption performance of hydrothermal carbon, and forms high-quality functional materials.
Smart Images

Figure CN119060749A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biochar, and particularly relates to a method for preparing biochar by continuous pyrolysis of Salix psammophila. Background Art
[0002] Salix psammophila is one of the most widely planted tree species in China's sandy wastelands. It not only provides windbreaks and sand fixation, but also grows rapidly, requiring only three to six years of harvesting. Its calorific value is comparable to that of coal, earning it the nickname "Green Sand Coalfield." Therefore, converting waste Salix psammophila into high-value biomass products is crucial. However, pyrolysis is currently the most common method. This process requires dry conditions, high temperatures and pressures, and produces large amounts of CO2 and harmful gases, leading to significant heat loss and significant disadvantages in promoting carbonization of the raw materials. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to address the deficiencies of the above-mentioned existing technologies and provide a method for preparing biochar by continuous pyrolysis of Salix psammophila. This method can utilize discarded Salix psammophila to prepare hydrothermal carbon by hydrothermal carbonization. The reaction process is relatively milder than the pyrolysis carbonization method, and there is no large amount of CO2 and harmful gas emissions. The prepared hydrothermal carbon has excellent adsorption performance.
[0004] In order to solve the above technical problems, the technical solution adopted in the present invention is: a method for preparing biochar by continuous pyrolysis of Salix psammophila, characterized in that the method is: the Salix psammophila is peeled, cleaned and dried, then cut into pieces, crushed and sieved to obtain Salix psammophila wood powder, which is then mixed with water and added to a polytetrafluoroethylene-lined hydrothermal reactor, and then heated to 230-290°C at a heating rate of 5°C / min for hydrothermal reaction, maintained for 24-48 hours, cooled to room temperature and filtered to obtain a solid product, the solid product is washed with anhydrous ethanol and deionized water until the filtrate is clear, and finally dried to obtain hydrothermal charcoal.
[0005] Preferably, it is sieved through an 80-mesh screen.
[0006] Preferably, the mass ratio of Salix psammophila wood powder to water is 1:30.
[0007] Preferably, the temperature of the hydrothermal reaction is 270° C. and maintained for 48 hours.
[0008] Compared with the prior art, the present invention has the following advantages:
[0009] 1. The present invention utilizes discarded Salix psammophila to prepare hydrothermal carbon by hydrothermal carbonization. As a high-quality fuel with high value, the reaction process is relatively milder than the pyrolysis carbonization method, and there is no large amount of CO2 and harmful gas emissions. The prepared hydrothermal carbon has excellent adsorption properties. During the hydrothermal reaction, the hemicellulose in Salix psammophila is dehydrated, decarboxylated, condensed, polymerized and aromatized to form micro-carbon balls of uneven size. The cellulose in Salix psammophila is pyrolyzed to produce carbon micro-balls and soluble lignin fragments and lignin crystal structure carbon. The hemicellulose and cellulose in Salix psammophila are both degraded. The final product is mainly a polyaromatic structure, followed by alkyl carbon, and new carboxyl and carbonyl functional groups are generated. The rich oxygen-containing functional groups can be used as functional materials for surface modification or composite with other materials.
[0010] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 These are SEM images of hydrothermal carbon produced in Example 1 of the present invention at different hydrothermal reaction temperatures.
[0012] Figure 2 The N2 adsorption / desorption isotherms and corresponding pore size distribution (PSD) curves of the hydrothermal carbon prepared at different reaction times in Example 2 of the present invention are shown.
[0013] Figure 3 1 is an infrared spectrum of hydrothermal carbon at different hydrothermal reaction temperatures according to Example 1 of the present invention.
[0014] Figure 4 The infrared spectra of hydrothermal carbon at different reaction times according to Example 2 of the present invention are shown.
[0015] Figure 5 1 is a Raman spectrum of hydrothermal carbon at different hydrothermal reaction temperatures in Example 1 of the present invention.
[0016] Figure 6 The Raman spectra of the hydrothermal carbon at different reaction times according to Example 2 of the present invention are shown. DETAILED DESCRIPTION
[0017] Example 1
[0018] The present embodiment discloses a method for preparing biochar by continuous pyrolysis of Salix psammophila, which comprises the following steps: peeling and cleaning the Salix psammophila and drying the same, then cutting and crushing the pieces through an 80-mesh sieve to obtain Salix psammophila wood powder, mixing the pieces with water in a mass ratio of 1:30, and adding the pieces to five groups of polytetrafluoroethylene-lined hydrothermal reactors, and then heating the pieces to 210°C, 230°C, 250°C, 270°C, and 290°C at a heating rate of 5°C / min for hydrothermal reaction, maintaining the temperature for 48 hours, and then cooling the pieces to room temperature and performing a filtration reaction. The solid product was filtered and washed with anhydrous ethanol and deionized water until the filtrate was clear, and finally dried to obtain hydrothermal carbon; the hydrothermal carbon obtained at a hydrothermal reaction temperature of 210°C was marked as SC210, the hydrothermal carbon obtained at a hydrothermal reaction temperature of 230°C was marked as SC230, the hydrothermal carbon obtained at a hydrothermal reaction temperature of 250°C was marked as SC250, the hydrothermal carbon obtained at a hydrothermal reaction temperature of 270°C was marked as SC270, and the hydrothermal carbon obtained at a hydrothermal reaction temperature of 290°C was marked as SC290.
[0019] Figure 1: This is an SEM picture of hydrothermal carbon at different hydrothermal reaction temperatures in this embodiment. It can be seen from the figure that at 210°C, a lot of micro-carbon balls with uniform particle size but smooth surface are produced. As the temperature rises, the number of micro-carbon balls increases and the particle size becomes larger. The micro-carbon balls produced at 210°C are produced by hemicellulose. Under mild (T<200°C) hydrothermal carbonization (HTC) conditions, hemicellulose is first decomposed into oligomers and then decomposed into monosaccharides of xylose, galactose, glucose and fructose. As the temperature rises, micro-carbon balls of uneven size are formed through liquid phase dehydration, decarboxylation, condensation, polymerization and aromatization. When the temperature rises to 220°C, cellulose also begins to decompose. When the temperature is >230°C, subcritical water can destroy the hydrogen bonds and crystal structure of cellulose and hydrolyze β-(1-4) glycosidic bonds to form glucose monomers. Cellulose solubilization products and hemicellulose hydrolysis products are typically highly reactive, undergoing condensation, oligomerization, and polymerization reactions that occur in parallel, ultimately leading to the formation of polymeric furanic and aromatic structures connected by lipid chains. When a precipitate forms on the cellulose surface, water access is inhibited. Consequently, cellulose undergoes pyrolysis rather than dissolution and hydrolysis, resulting in carbonaceous materials with aromatic structures rather than furanic materials. Lignin, also a major component of lignocellulosic biomass, has a relatively low degradation rate, with phenolic compounds such as phenol, methoxyphenol, and catechol being the primary products during HTC. Lignin is a high-molecular-weight, cross-linked polymer that decomposes slowly throughout the HTC process within the decomposition temperature range (200-500°C). Soluble lignin fragments rapidly aggregate, and some stable lignin crystal structures may undergo demethylation and pyrolysis rather than fragmentation. During HTC, especially under mild conditions, lignin undergoes minor chemical and physical changes. When the temperature reaches above 250°C, the degradation products (such as furans, ketones and phenolic compounds) from the amorphous part (hemicellulose and soluble lignin) can undergo isomerization, dehydration, fragmentation and condensation reactions. These substances will precipitate on the cellulose surface, inhibiting water from entering the cellulose, preventing its degradation and forming carbon-like precipitates in the hydrothermal fluid. Therefore, the part with increased microcarbon balls is formed by the pyrolysis of hemicellulose, cellulose and soluble lignin, and the carbonaceous material with no microcarbon ball morphology is formed by cellulose and stable lignin crystal structure.
[0020] Table 1 Chemical composition of Salix psammophila and hydrothermal charcoal prepared in Example 1
[0021]
[0022] From the data in Table 1, it can be seen that when the hydrothermal reaction was carried out at 210°C, almost all the hemicellulose in the Salix psammophila was greatly degraded. When treated at 250°C, glucose and hemicellulose sugars were no longer detectable, which means that the hemicellulose and cellulose almost completely underwent hydrothermal degradation reaction. After the hydrothermal reaction, the content of clason lignin was significantly increased to varying degrees.
[0023] Table 2 Industrial analysis and energy characteristics of Salix psammophila and hydrothermal charcoal with different hydrothermal reaction times
[0024]
[0025] The data in Table 2 show that as temperature increases, mass yield and energy production decrease, while energy density increases. The mass yield and energy production of Salix psammophila show a particularly pronounced trend, initially decreasing rapidly before plateauing, with a correspondingly high rate of increase in energy density. This suggests that temperature is a significant factor.
[0026] Example 2
[0027] The present embodiment discloses a method for preparing biochar by continuous pyrolysis of Salix psammophila, which comprises the following steps: peeling and cleaning the Salix psammophila and drying the same, then cutting and crushing the pieces through an 80-mesh sieve to obtain Salix psammophila wood powder, mixing the pieces with water in a mass ratio of 1:30, and adding the pieces to seven groups of polytetrafluoroethylene-lined hydrothermal reactors, and then heating the mixture to 270°C at a heating rate of 5°C / min for hydrothermal reaction, maintaining the mixture for 2h, 4h, 8h, 12h, 16h, 24h, and 48h, respectively, cooling the pieces to room temperature, filtering the pieces, and obtaining a solid product. The solid product is then precipitated with anhydrous ethanol. and deionized water until the filtrate is clear, and finally dried to obtain hydrothermal charcoal; the hydrothermal charcoal obtained within a hydrothermal reaction time of 2 h is marked as SC2h, the hydrothermal charcoal obtained within a hydrothermal reaction time of 4 h is marked as SC4h, the hydrothermal charcoal obtained within a hydrothermal reaction time of 8 h is marked as SC8h, the hydrothermal charcoal obtained within a hydrothermal reaction time of 12 h is marked as SC12h, the hydrothermal charcoal obtained within a hydrothermal reaction time of 16 h is marked as SC16h, the hydrothermal charcoal obtained within a hydrothermal reaction time of 24 h is marked as SC24h, and the hydrothermal charcoal obtained within a hydrothermal reaction time of 28 h is marked as SC48h.
[0028] Table 5 Industrial analysis and energy characteristics of Salix psammophila and hydrothermal charcoal at different hydrothermal reaction times
[0029]
[0030] Figure 2The N2 adsorption / desorption isotherms and corresponding pore size distribution (PSD) curves of hydrothermal carbon prepared at different reaction times in Example 2 of the present invention. The specific surface area and PSD were calculated using the Brunauer-Emmett-Teller (BET) method and the Barrett-Joyner-Halenda (BJH) method, respectively. The isotherm of the hydrothermal carbon is a typical type IV isotherm with a hysteresis loop, indicating the presence of micropores and mesopores. From the enlarged illustration of the BJH pore size distribution in (b), it can be seen that the hydrothermal carbon is rich in micropores. The isotherm shows significant hysteresis characteristics at relatively high pressure (P / P0=0.0-1.0), indicating the presence of abundant mesopores. Therefore, the Salix psammophila biochar exhibits a highly developed hierarchical pore network of micropores and mesopores. At the same time, in the PSD curve, the slightly upward trend of the curve above 50nm corresponds to the presence of large pores caused by the accumulation of carbon particles.
[0031] PSD data indicate that the majority of pores in the hydrothermal carbon are <2 nm in size. A clear upward-trending peak (<2 nm) further confirms the abundant micropores in the hydrothermal carbon. The specific surface area ranges from 5.56 to 18.346 m² g⁻¹, and the total pore volume ranges from 0.023 to 0.075 cm³ g⁻¹. SCn exhibits the largest specific surface area, while YCn and ZCn exhibit similar pore volumes. Both the specific surface area and pore volume are highest at 210°C. As the temperature increases, the specific surface area and pore volume decrease, with minimal change.
[0032] Figure 3 It is the infrared spectrum of hydrothermal carbon at different hydrothermal reaction temperatures. Figure 4 The infrared spectra of hydrothermal carbon at different reaction times are shown in Figure 2. The hydrothermal carbon of each biomass component contains OH groups (at 3700-3000 cm -1 Because some hydroxyl groups in the original cellulose undergo dehydration reaction, the intensity of hydrothermal carbon is much lower than that of the raw material components. -1 The aliphatic CH singlet peaks are at 2970 and 2930 cm -1 A small double vibration peak of aliphatic CH bond (mainly methylene bridge) is formed on the left and right. With the increase of reaction temperature and time, the peak gradually weakens and shifts to a higher wave number, indicating that the active ketone group has undergone a certain reaction and turned into an in-plane stretching vibration peak of CH. -1 There is an obvious peak around 1740cm -1 The left and right sides show the non-conjugated carbonyl (C=O) stretching vibration absorption peak in the chromophore of hemicellulose polyxylose. As the temperature rises and the time increases in the hydrothermal carbonization material, the decarboxylation reaction occurs and the product is converted into CO2. This peak no longer exists, indicating that the hemicellulose has been completely degraded during the hydrothermal carbonization process. -1New peaks are formed around 1510cm, indicating that new functional groups such as ketone, carboxyl or ester groups are formed in the hydrothermal carbon, and they move to lower wavenumbers with the extension of reaction time and the increase of temperature. -1 and 1460cm -1 The peaks on the left and right represent the C=C stretching vibration absorption peak in the aromatic ring of lignin and the -CH2 deformation vibration absorption peak on the skeleton. These peaks gradually disappear at 1600cm -1 and 1452cm -1 A new stretching vibration peak is formed at the center, which corresponds to the stretching vibration of the aromatic ring skeleton C=C and the in-plane bending vibration peak caused by the CH chain of the aliphatic, methylene and methyl groups.
[0033] The 1050 cm-1 region is observed in the cellulose, hemicellulose, and lignin structures of all biomasses. -1 Symmetrical CO stretching vibration at 1050 cm -1 The peaks on the left and right come from the CO stretching vibration peaks of ester groups, phenols and fatty alcohols. They completely disappear after the hydrothermal reaction, indicating that the CO chain is broken due to decarboxylation. Assigned to 1300-950cm -1 There are many CO stretching vibration peaks, such as 1044cm -1 and 1114cm -1 The peak appears in hydrochar. In cellulose and hemicellulose, the CO bonds are ether bonds, while in lignin, the CO bonds are methoxy or ether bonds. This indicates that the methoxy and ether bonds are easily broken during the HTC process. In almost all biomass samples, the G (guaiac) units of lignin are partially degraded, which can be seen by the peak at 1276 cm -1 Observe the decrease in vibration intensity at 650-950cm -1 New aromatic rings or twisted C-H bonds in aromatic compounds appear, but the strength increases with increasing temperature. The results show that a cross-linked network structure of the fibers has been formed, and the aromatic ring structure of this carbon network gradually strengthens with increasing temperature. The above analysis shows that compared with unreacted lignocellulose, the prepared hydrothermal carbon is composed of a complex aromatic structure, with a large number of oxygen-containing functional groups such as ether and phenolic hydroxyl groups, and a significantly lower alkane content, confirming the occurrence of degradation, polymerization, and aromatization reactions.
[0034] To confirm the presence of aromatic carbon on the hydrocarbons, Raman spectroscopy measurements were performed. Figure 5 It is the Raman spectrum of hydrothermal carbon at different hydrothermal reaction temperatures. Figure 6 The Raman spectra of hydrothermal carbon at different reaction times are shown in Figure 2. -1 and 1595cm -1 There are two main bands on the left and right, which can be attributed to the D band (sp 3) and G band (sp 2 ). Usually, D band represents sp 3 The vibration mode of carbon atoms in hybrid orbitals, G bands are related to the vibration mode of sp2 carbon atoms. The ratio of ID and IG bands in the hydrothermal carbonization product of Salix psammophila from 2.01 to 1.68 and in the hydrothermal carbonization product of Salix psammophila from 1.65 to 1.34 respectively, revealing the presence of C (sp) in the condensed benzene ring of benzene or amorphous amorphous carbon. 2 ) atoms. Therefore, small aromatic clusters must exist in the hydrocarbon sample. The presence of aromatic structures in the hydrothermal carbonization products is confirmed. A higher ID / IG ratio means that the hydrothermal carbon will produce larger carbon structure defects, which has great application prospects in the fields of adsorption or energy storage. The shift of the D and G band peak positions is due to the broadening of the D band and the different bond vibration modes present in the sample. When the HTC process changes the surface chemistry of carbonized lignocellulose, these bonds resonate at their respective wavelengths. The changes in ID / IG at different temperatures indicate that the content and type of surface functional groups introduced by the hydrothermal carbonization process are also different, which also confirms that the degree of functionalization of different substances in the hydrothermal process is also different.
[0035] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent variation made to the above embodiment based on the essence of the invention technology shall still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for preparing biochar by continuous pyrolysis of Salix psammophila, characterized in that: The method comprises the following steps: peeling and cleaning the salix psammophila, drying the salix psammophila, cutting into pieces, crushing and screening to obtain salix psammophila wood powder, mixing the salix psammophila wood powder with water and adding the salix psammophila wood powder to a polytetrafluoroethylene-lined hydrothermal reactor, and then heating the salix psammophila wood powder to 230-290°C at a heating rate of 5°C / min for hydrothermal reaction, maintaining the temperature for 24-48 hours, cooling the salix psammophila wood powder to room temperature, filtering the salix psammophila wood powder to obtain a solid product, washing the solid product with anhydrous ethanol and deionized water until the filtrate is clear, and finally drying the charcoal to obtain hydrothermal charcoal.
2. The method for preparing biochar by continuous pyrolysis of Salix psammophila according to claim 1, characterized in that: Pass through 80 mesh sieve.
3. The method for preparing biochar by continuous pyrolysis of Salix psammophila according to claim 1, characterized in that: The mass ratio of Salix psammophila wood powder to water is 1:
30.
4. The method for preparing biochar by continuous pyrolysis of Salix psammophila according to claim 1, characterized in that: The temperature of the hydrothermal reaction was 270°C and maintained for 48 h.