Converter smelting method of extremely low phosphorus steel
The converter smelting method for ultra-low phosphorus steel addresses production challenges by using pretreated molten iron, slag blocking, and controlled secondary smelting to achieve stable, low-phosphorus steel production.
Patent Information
- Application Number
- CN202411182994.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The challenge of producing low-phosphorus steel is exacerbated by the use of high-phosphorus ores and blast furnace smelting technologies, leading to early slagging difficulties and poor dephosphorization effects, making it difficult to achieve stable production of steel with low phosphorus content.
A converter smelting method involving pretreated molten iron, slag blocking, addition of lime and aluminum-manganese iron, and secondary smelting with controlled oxygen blowing and material addition to achieve ultra-low phosphorus steel.
The method stabilizes the phosphorus content below 0.005% and ensures a controllable, adaptable process flow suitable for industrial application.
Smart Images

Figure BDA0005012744230000081 
Figure BDA0005012744230000082 
Figure BDA0005012744230000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of converter smelting of extremely low-phosphorus steel, and relates to a converter smelting method of extremely low-phosphorus steel. Background Art
[0002] Phosphorus is a harmful element in most steel grades, which will reduce the plasticity and toughness of steel. This phenomenon is more obvious at low temperatures. The industry usually calls it the "cold brittleness" phenomenon. Phosphorus should be removed as much as possible during the smelting process. Converter steelmaking is the most economical and effective reaction unit for removing phosphorus from steel. However, with the commissioning of a large number of high-phosphorus ores and the development of blast furnace ironmaking technology, the blast furnace low-silicon hot metal smelting technology has matured. As the production proportion of low-silicon and high-phosphorus hot metal increases, low-silicon and high-phosphorus hot metal is prone to early slagging difficulties, process drying, and poor process dephosphorization effects during converter smelting. These problems are more prominent, which brings certain difficulties to the converter production of low-phosphorus steel.
[0003] Therefore, how to find a more suitable way to solve the above-mentioned technical problems existing in the existing process has become one of the urgent problems to be solved by many front-line researchers in the industry. Summary of the invention
[0004] In view of this, the technical problem to be solved by the present invention is to provide a converter smelting method for extremely low-phosphorus steel. The method for smelting low-phosphorus steel provided by the present invention achieves the purpose of stably producing low-phosphorus steel in a converter, and can stably control the phosphorus content of steel tapped from the converter to be below 0.005%. Moreover, the process flow is simple, controllable, and adaptable, and is more suitable for industrial promotion and application.
[0005] The present invention provides a converter smelting method for ultra-low phosphorus steel, comprising the following steps:
[0006] 1) The molten iron is put into the furnace for converter smelting, and then the molten steel is obtained after the slag is blocked and the lime and aluminum-manganese iron are added with the steel flow;
[0007] 2) The molten steel obtained in the above steps is added with molten iron and then put into the furnace again for secondary converter smelting to obtain ultra-low phosphorus steel.
[0008] Preferably, the molten iron is molten iron that has been pretreated outside the furnace;
[0009] The pretreatment includes desulfurization and slagging steps.
[0010] Preferably, the terminal temperature of the converter smelting is 1620-1640°C;
[0011] The mass content of phosphorus at the end point of converter smelting is less than or equal to 0.020%.
[0012] Preferably, the amount of lime added is 6-8 kg / t;
[0013] The amount of aluminum-manganese iron added is 2.0-2.5 kg / t.
[0014] Preferably, the amount of molten iron added is 0.05-0.08 kg / t;
[0015] The molten iron in step 2) is specifically molten iron that has been pretreated outside the furnace.
[0016] Preferably, before the re-entry into the furnace, the step of pouring out the slag in the converter furnace is also included;
[0017] The blowing gun position of the secondary smelting is 1400-1500mm.
[0018] Preferably, the blowing oxygen pressure of the secondary smelting is 0.82-0.87 MPa;
[0019] In the secondary smelting, lime, dolomite and ore are added within 1 minute after the start of blowing;
[0020] The ore includes sintered ore.
[0021] Preferably, in the secondary smelting, the amount of lime added is 20-25 kg / t;
[0022] In the secondary smelting, the amount of dolomite added is 5-7 kg / t;
[0023] In the secondary smelting, the amount of ore added is 0-5 kg / t.
[0024] Preferably, in the secondary smelting, after blowing for 1 to 4 minutes, the temperature of the molten steel is measured, the carbon content of the molten steel is measured, and a sample is taken for testing of the phosphorus content;
[0025] The oxygen blowing amount and the ore adding amount are dynamically controlled according to one or more of the temperature, carbon content and phosphorus content of the molten steel.
[0026] Preferably, the terminal temperature of the secondary converter smelting is 1610-1625°C;
[0027] The mass content of carbon in the molten steel at the end point of the secondary converter smelting is 0.04% to 0.07%;
[0028] The mass content of phosphorus in the molten steel at the end point of the secondary converter smelting is less than or equal to 0.005%.
[0029] The present invention provides a converter smelting method for ultra-low phosphorus steel, comprising the following steps: first, molten iron is put into a furnace for converter smelting, then molten steel is obtained after slag blocking and steel is tapped and lime and aluminum-manganese iron are added with the steel flow; then, molten iron is added to the molten steel obtained in the above steps and then put into the furnace again for secondary converter smelting to obtain ultra-low phosphorus steel. Compared with the prior art, the present invention designs a converter smelting method for ultra-low phosphorus steel with specific steps. The present invention is not affected by the ratio of raw materials entering the furnace, the phosphorus content of molten iron, etc. The converter smelting process is easy to control, and the final carbon and phosphorus content are easy to reach the required range. Moreover, the process flow is simple, controllable, and adaptable, and it is more suitable for industrial promotion and application.
[0030] The smelting method of the ultra-low phosphorus steel provided by the present invention can effectively ensure the dephosphorization effect of the converter, achieve the purpose of stably producing low-phosphorus steel in the converter, and can stably control the phosphorus content of the final steel tapped from the converter to be below 0.005%. DETAILED DESCRIPTION
[0031] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention rather than limiting the patent claims of the present invention.
[0032] All raw materials of the present invention are not particularly limited in their sources and can be purchased from the market or prepared according to conventional methods well known to those skilled in the art.
[0033] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses industrial purity or conventional purity in the field of low-phosphorus steel smelting.
[0034] The brands and abbreviations of all raw materials of the present invention are conventional brands and abbreviations in the art. Each brand and abbreviation is clear and definite in the field of its related use. Those skilled in the art can purchase them from the market or prepare them by conventional methods according to the brands, abbreviations and corresponding uses.
[0035] The present invention provides a converter smelting method for ultra-low phosphorus steel, comprising the following steps:
[0036] 1) The molten iron is put into the furnace for converter smelting, and then the molten steel is obtained after the slag is blocked and the lime and aluminum-manganese iron are added with the steel flow;
[0037] 2) The molten steel obtained in the above steps is added with molten iron and then put into the furnace again for secondary converter smelting to obtain ultra-low phosphorus steel.
[0038] The invention firstly puts molten iron into a furnace for converter smelting, then taps out steel through slag blocking and adds lime and aluminum-manganese iron with the steel flow to obtain molten steel.
[0039] In the present invention, the molten iron is preferably molten iron that has been pretreated outside the furnace.
[0040] In the present invention, the pretreatment preferably includes desulfurization and slag removal steps. Specifically, the desulfurization and slag removal steps can be KR desulfurization, adding a desulfurizer to the iron ladle, stirring desulfurization, and then slag removal.
[0041] In the present invention, the terminal temperature of the converter smelting is preferably 1620-1640°C, more preferably 1624-1636°C, and more preferably 1628-1632°C.
[0042] In the present invention, the mass content of phosphorus at the end point of converter smelting is preferably less than or equal to 0.020%.
[0043] In the present invention, the amount of lime added is preferably 6-8 kg / t, more preferably 6.4-7.6 kg / t, and more preferably 6.8-7.2 kg / t.
[0044] In the present invention, the addition amount of the aluminum-manganese ferro is preferably 2.0-2.5 kg / t, more preferably 2.1-2.4 kg / t, more preferably 2.2-2.3 kg / t. Specifically, the content and composition requirements of the aluminum-manganese ferro in the present invention, by mass percentage, can be: Al≥53%, Mn≥4.5%, Si≤1.5%, P≤0.07%, S≤0.07%.
[0045] The present invention further adds molten iron to the molten steel obtained in the above steps and puts the molten steel into the furnace again for secondary converter smelting to obtain ultra-low phosphorus steel.
[0046] In the present invention, the amount of molten iron added is preferably 0.05-0.08 kg / t, more preferably 0.055-0.075 kg / t, and more preferably 0.06-0.07 kg / t.
[0047] In the present invention, the molten iron in step 2) is preferably molten iron that has been pretreated outside the furnace.
[0048] In the present invention, before re-entering the furnace, it is preferred that the step of pouring out the slag in the converter furnace is included.
[0049] In the present invention, the blowing lance position of the secondary smelting is preferably 1400-1500 mm, more preferably 1420-1480 mm, and more preferably 1440-1460 mm.
[0050] In the present invention, the blowing oxygen pressure of the secondary smelting is preferably 0.82-0.87 MPa, more preferably 0.83-0.86 MPa, and more preferably 0.84-0.85 MPa.
[0051] In the present invention, the secondary smelting preferably adds lime, dolomite and ore within 1 minute after the start of blowing;
[0052] In the present invention, the ore preferably includes sintered ore.
[0053] In the present invention, in the secondary smelting, the amount of lime added is preferably 20-25 kg / t, more preferably 21-24 kg / t, and more preferably 22-23 kg / t.
[0054] In the present invention, in the secondary smelting, the amount of dolomite added is preferably 5-7 kg / t, more preferably 5.4-6.6 kg / t, more preferably 5.8-6.2 kg / t.
[0055] In the present invention, in the secondary smelting, the amount of ore added is preferably 0-5 kg / t, more preferably 1-4 kg / t, and more preferably 2-3 kg / t.
[0056] In the present invention, in the secondary smelting, after blowing for 1 to 4 minutes (or 2 to 3 minutes), it is preferred to measure the temperature of the molten steel, measure the carbon content of the molten steel, and take samples for phosphorus content. Specifically, the secondary gun TSC probe is used to measure the temperature and carbon and take samples.
[0057] In the present invention, it is preferred to dynamically control the oxygen blowing amount and the amount of ore added according to one or more of the temperature, carbon content and phosphorus content of the molten steel. In the present invention, the oxygen blowing amount is controlled according to the temperature and carbon content. In this method, the carbon content will not be too high, so it is not considered. The temperature is based on the oxygen blowing amount of 100Nm 3 Increase by about 10℃. Ore is generally not added unless the temperature is too high, then the temperature can be reduced by about 30℃ per 1000kg.
[0058] In the present invention, the terminal temperature of the secondary converter smelting is preferably 1610-1625°C, more preferably 1613-1622°C, and more preferably 1616-1619°C.
[0059] In the present invention, the mass content of carbon in the molten steel at the end point of the secondary converter smelting is preferably 0.04% to 0.07%, more preferably 0.045% to 0.065%, and more preferably 0.05% to 0.06%.
[0060] In the present invention, the mass content of phosphorus in the molten steel at the end point of the secondary converter smelting is preferably less than or equal to 0.005%.
[0061] The present invention is to complete and refine the overall technical solution and further improve the dephosphorization effect. The converter smelting method of the ultra-low phosphorus steel may specifically include the following contents:
[0062] The present invention provides a smelting method of extremely low phosphorus steel, which can effectively ensure the dephosphorization effect of the converter and stabilize the final phosphorus content of the converter below 0.005%. The technical solution is as follows:
[0063] 1. Pretreatment of molten iron outside the furnace;
[0064] 2. The molten iron is put into the furnace for conventional smelting, the final temperature of the converter is controlled at 1620-1640°C, and the final phosphorus is controlled below 0.020%;
[0065] 3. The converter is tapped with slag blocking, and 6-8 kg / t lime and 2.0-2.5 kg / t aluminum-manganese iron are added into the steel flow during tapping;
[0066] 4. After the steel is tapped, the molten steel is transferred to the raw material bay and mixed with 0.05-0.08 kg / t molten iron;
[0067] 5. Put the molten steel mixed with molten iron directly into the furnace for secondary smelting; pour out all the slag in the converter before entering the furnace.
[0068] 6. Secondary smelting adopts the following methods:
[0069] (1) Blowing gun position: 1400-1500mm, oxygen pressure: 0.82-0.87Mpa. Add 20-25kg / t of lime, 5-7kg / t of dolomite and 0-5kg / t of ore at one time within 1 minute after blowing.
[0070] (2) Use the auxiliary gun to measure TSC at about 2 minutes of blowing;
[0071] (3) Dynamically control the oxygen blowing amount and ore addition amount based on TSC measurement data.
[0072] (4) End point control:
[0073] End point temperature: 1610~1625℃, end point carbon: 0.04~0.07%.
[0074] The present invention provides a converter smelting method for ultra-low phosphorus steel. The converter smelting method for ultra-low phosphorus steel with specific steps designed by the present invention is not affected by the ratio of raw materials entering the furnace, the phosphorus content of molten iron, etc. The converter smelting process is easy to control, and the final carbon and phosphorus content are easy to reach the required range. Moreover, the process flow is simple, the controllability is good, the adaptability is strong, and it is more suitable for industrial promotion and application.
[0075] The smelting method of the ultra-low phosphorus steel provided by the present invention can effectively ensure the dephosphorization effect of the converter, achieve the purpose of stably producing low-phosphorus steel in the converter, and can stably control the phosphorus content of the final steel tapped from the converter to be below 0.005%.
[0076] In order to further illustrate the present invention, a converter smelting method for ultra-low phosphorus steel provided by the present invention is described in detail below in combination with embodiments. However, it should be understood that these embodiments are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the following embodiments.
[0077] Example
[0078] The smelting method of the ultra-low phosphorus steel disclosed in the embodiment of the present invention comprises the following steps:
[0079] 1. Pretreatment of molten iron outside the furnace;
[0080] 2. The molten iron is put into the furnace for conventional smelting, the final temperature of the converter is controlled at 1620-1640°C, and the final phosphorus is controlled below 0.020%.
[0081] The control of the final temperature and final phosphorus of the converter smelting in Examples 1 to 6 is shown in Table 1. Table 1 is a statistical table of the control of the final temperature and final phosphorus of the converter smelting in Examples 1 to 6 of the present invention.
[0082] Table 1
[0083] Serial number End point temperature / ℃ End point phosphorus content / % Example 1 1630 0.020 Example 2 1636 0.018 Example 3 1630 0.019 Example 4 1622 0.015 Example 5 1631 0.017 Example 6 1628 0.019
[0084] 3. The converter is tapped with slag blocking. When tapping, 6-8 kg / t lime and 2.0-2.5 kg / t aluminum-manganese iron are added into the steel flow;
[0085] 4. After the steel is tapped, the molten steel is transferred to the raw material bay and mixed with 0.05-0.08 kg / t molten iron;
[0086] The amounts of lime, aluminum-manganese-iron and molten steel added to molten iron when tapping steel in Examples 1 to 6 are shown in Table 2. Table 2 is a statistical table of the amounts of lime, aluminum-manganese-iron and molten steel added to molten iron when tapping steel in the embodiments of the present invention.
[0087] Table 2
[0088] Serial number Lime addition amount / (kg / t) Amount of aluminum-manganese-iron added / (kg / t) Amount of molten iron added / (kg / t) Example 1 6.8 2.2 0.05 Example 2 7.5 2.3 0.06 Example 3 7 2.0 0.08 Example 4 7.8 2.5 0.06 Example 5 8.0 2.2 0.07 Example 6 7.6 2.3 0.06
[0089] 5. Put the molten steel mixed with molten iron directly into the furnace for secondary smelting; pour out all the slag in the converter before entering the furnace.
[0090] 6. Secondary smelting adopts the following methods:
[0091] (1) Blowing gun position: 1400-1500 mm, oxygen pressure: 0.82-0.87 MPa, add lime 20-25 kg / t; dolomite 5-7 kg / t; ore 0-5 kg / t at one time within 1 minute after blowing. The specific oxygen supply process parameters and bulk material addition of secondary smelting of Examples 1-6 are shown in Table 3. Table 3 is a statistical table of specific oxygen supply process parameters and bulk material addition of secondary smelting of Examples 1-6 of the present invention.
[0092] Table 3
[0093]
[0094] (2) Use the auxiliary gun to measure TSC at about 2 minutes of blowing;
[0095] (3) Dynamically control the oxygen blowing amount and ore addition amount based on TSC measurement data;
[0096] (4) End point control
[0097] The end point temperature: 1610-1625°C, the end point carbon: 0.04-0.07%; the statistics of the temperature measurement, carbon determination and sampling and testing of phosphorus content of the end point control auxiliary gun TSO of Examples 1-6 are shown in Table 4. Table 4 is a statistical table of the temperature measurement, carbon determination and sampling and testing of phosphorus content of the end point control auxiliary gun TSO of Examples 1-6 of the present invention.
[0098] Table 4
[0099]
[0100]
[0101] The above is a detailed introduction to the converter smelting method of an ultra-low phosphorus steel provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A converter smelting method for ultra-low phosphorus steel, characterized in that: The following steps are involved: 1) The molten iron is put into the furnace for converter smelting, and then the molten steel is obtained after the slag is blocked and the lime and aluminum manganese iron are added with the steel flow; 2) The molten steel obtained in the above steps is added with molten iron and then put into the furnace again for secondary converter smelting to obtain ultra-low phosphorus steel.
2. The method according to claim 1, characterized in that The molten iron is specifically molten iron that has been pretreated outside the furnace; The pretreatment includes desulfurization and slagging steps.
3. The method according to claim 1, characterized in that The final temperature of the converter smelting is 1620-1640°C; The mass content of phosphorus at the end point of converter smelting is less than or equal to 0.020%.
4. The method according to claim 1, characterized in that: The amount of lime added is 6-8 kg / t; The amount of aluminum-manganese iron added is 2.0-2.5 kg / t.
5. The method according to claim 1, characterized in that The amount of molten iron added is 0.05-0.08 kg / t; The molten iron in step 2) is specifically molten iron that has been pretreated outside the furnace.
6. The method according to claim 1, characterized in that Before the furnace is put back into the furnace, the step of pouring out the slag in the converter furnace is also included; The blowing gun position of the secondary smelting is 1400-1500mm.
7. The method according to claim 1, characterized in that The blowing oxygen pressure of the secondary smelting is 0.82-0.87Mpa; In the secondary smelting, lime, dolomite and ore are added within 1 minute after the start of blowing; The ore includes sintered ore.
8. The method according to claim 7, characterized in that In the secondary smelting, the amount of lime added is 20-25 kg / t; In the secondary smelting, the amount of dolomite added is 5-7 kg / t; In the secondary smelting, the amount of ore added is 0-5 kg / t.
9. The method according to claim 1, characterized in that: In the secondary smelting, after blowing for 1 to 4 minutes, the temperature of the molten steel is measured, the carbon content of the molten steel is measured, and the phosphorus content is sampled and tested; The oxygen blowing amount and the ore adding amount are dynamically controlled according to one or more of the temperature, carbon content and phosphorus content of the molten steel.
10. The method according to claim 9, characterized in that The terminal temperature of the secondary converter smelting is 1610-1625°C; The mass content of carbon in the molten steel at the end point of the secondary converter smelting is 0.04% to 0.07%; The mass content of phosphorus in the molten steel at the end point of the secondary converter smelting is less than or equal to 0.005%.