Composite binder for granulating fine-grained titanium-rich material and granulating method
By using composite binder of silicate and boiling chlorination dust collecting slag and granulation of fine-grained titanium-rich material, the problem of groove flow and surge during boiling chlorination is solved, and the problem of fine-grained titanium-rich material is achieved. High-efficiency granulation and boiling chlorination furnaces with good stability reduce titanium resource waste and production costs.
Patent Information
- Application Number
- CN202411201665.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
During the boiling chlorination process, fine-grained titanium-rich material can easily lead to groove flow and rush, resulting in low boiling chlorination rate. The existing fine-grained titanium-rich material binder cannot meet the industrial production requirements, resulting in waste of titanium resources.
Provide a composite binder, including silicate and boiling chlorinated dust collecting slag, for granulation with fine-grained titanium-rich material, and obtain particle size by granulation methods such as fluidized beds, discs, V-shaped mixers, etc. Particles between 96μm and 900μm meet the requirements of boiling chlorination furnace entry.
It realizes efficient granulation of fine-grained titanium-rich materials, the product has good cold strength and thermal strength, good stability, meets the requirements of boiling chlorination process, and realizes solid waste recycling and reduces production costs.
Smart Images

Figure BDA0005017992250000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium resource utilization, and in particular relates to a composite binder used for granulating fine titanium-rich materials and a granulating method. Background Art
[0002] The main products of the titanium industry are titanium dioxide and titanium sponge. Titanium dioxide is mainly composed of titanium dioxide, which has high whiteness, good dispersibility and good hiding power. It is a high-quality white inorganic pigment and is widely used in coatings, plastics, papermaking, printing and dyeing and other industries. Titanium alloys have the advantages of light weight, high strength and corrosion resistance. They are widely used in medical equipment, aerospace, military industry and other fields. Titanium sponge is an important raw material for the production of titanium alloys. TiCl4 is an important intermediate product in the production of titanium dioxide and titanium sponge. The boiling chlorination method can accelerate the mass transfer and heat transfer process between the gas-solid phase. It has a short process flow, high production capacity and low environmental pollution. It has become the preferred method for preparing TiCl4.
[0003] China is a country with abundant titanium resources, accounting for 28% of the world's total. Titanium resources in nature are mainly vanadium-titanium magnetite, ilmenite and rutile. The grade of titanium in vanadium-titanium magnetite is low, and it coexists with various elements such as Fe, V, Mn, Cu, etc., which are difficult to separate by ore dressing methods. Natural rutile reserves are small, the ore structure is dense, the composition is complex, the particle size is fine, and the selectivity is poor. Ilmenite is often used to prepare artificial rutile, but it has high content of impurities such as calcium and magnesium. At present, acid leaching is often used to remove harmful impurities, but it will cause more than 80% of particles with a particle size of less than 96μm. The boiling chlorination method has high requirements for the quality of titanium-rich materials entering the furnace, TiO2 ≥ 90%, MgO + CaO < 1.5%, and particles with a particle size distribution between 96μm-900μm account for more than 90%. Fine-grained titanium-rich materials are prone to channeling, slugging, and large amount of fine particles escaping during the boiling chlorination process, resulting in low boiling chlorination rate, insufficient reaction of the charge, and serious impact on the smooth progress of the boiling chlorination process. The existing enrichment and titanium extraction and impurity removal process results in a large proportion of fine-grained titanium-rich materials, which cannot directly enter the boiling chlorination furnace. Therefore, the fine-grained titanium-rich materials must be granulated to meet the requirements of the boiling chlorination furnace for raw materials.
[0004] To address this issue, current research at home and abroad is mainly conducted from two aspects: granulation method and binder. Binder is the key factor that determines the granulation effect. Any granulation method requires the use of binder. Therefore, the research on binder is particularly important.
[0005] The binders used in the granulation of fine titanium-rich materials are divided into organic binders, inorganic binders and composite binders. The reaction temperature in the boiling chlorination furnace is between 900 and 1100 ° C. The heat resistance of organic binders is poor. They are prone to decomposition under high temperature conditions, resulting in the production of powdery particles. At the same time, the cost of organic binders is relatively high. The steps of composite binders are complicated in actual operation, and the material is easily crushed during the destruction stage. The fine particles need to be collected again and granulated again, which not only reduces efficiency but also increases costs. In addition, high molecular hydrocarbons with a wide range of structural changes composed of organic chemicals, such as heavy petroleum oil, asphalt, coal tar, coal tar, etc., are widely used in the composite research of binders for titanium-rich materials. In the sintering process, these high molecular compounds may release harmful gases, which have a greater negative impact on the environment. The raw materials of inorganic binders are easy to obtain, cheap, and have excellent high temperature resistance. The granulated products are relatively stable in the boiling chlorination furnace, but a large amount needs to be added, which affects the quality of the product. Summary of the invention
[0006] In view of the problem in the prior art that "the titanium-rich material particles are too fine to be directly used in a boiling chlorination furnace, resulting in a large waste of titanium resources, and at the same time, the existing fine-grained titanium-rich material binders cannot meet the requirements of industrial production", the purpose of the present invention is to provide a composite binder and a granulation method for granulating fine-grained titanium-rich materials, which are used to prepare boiling chlorination furnace charges whose composition, particle size and particle strength meet the requirements.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The invention provides a composite binder for granulating fine titanium-rich materials, comprising silicate and boiling chlorinated dust collecting residue, wherein the mass ratio of the silicate to the boiling chlorinated dust collecting residue is 1-10:1.
[0009] In a preferred embodiment, the silicate is an alkali metal silicate, preferably sodium silicate or potassium silicate.
[0010] In a preferred embodiment, the boiling chlorinated dust collecting residue comprises the following components, and the mass percentage of each component is:
[0011] Fe 5~11wt%; Al 1~3wt%; Ti5~9wt%; Mn 3~15wt%; Si 1~8wt%; Mg 1~5wt%; Ca 1~5wt%; C 30~50wt%; Cl 30~40wt%.
[0012] The present invention also provides a method for granulating fine-grained titanium-rich material, comprising the following steps:
[0013] (1) Preparation of composite adhesive: Weigh the adhesives according to a set ratio and mix them evenly to obtain a composite adhesive.
[0014] (2) Mixing fine-grained titanium-rich materials: Fully mix the prepared composite binder with the fine-grained titanium-rich materials. Weigh a certain proportion of water and add it to the fine-grained titanium-rich materials that have been mixed evenly to fully mix the fine-grained titanium-rich materials, the composite binder and the water.
[0015] (3) Granulation: The uniformly mixed fine-grained titanium-rich material granulation raw materials are placed into a granulation device, and the granulation product is obtained after drying.
[0016] Furthermore, in the step (1), the added amount of the composite binder is 0.2 to 3 wt% of the mass of the fine-grained titanium-rich material.
[0017] Furthermore, in the step (2), the fine-grained titanium-rich material refers to high-titanium slag, artificial rutile, or natural rutile with a particle size less than 96 μm.
[0018] Furthermore, in the step (2), the amount of water added is 10 to 30 wt % of the mass of the fine-grained titanium-rich material.
[0019] Furthermore, in the step (2), water is added to the raw materials in the form of a spray and mixed evenly.
[0020] Furthermore, in the step (3), the granulation method of the fine titanium-rich material includes fluidized bed granulation method, disc granulation method, V-type mixer granulation method and high-speed stirring granulation method.
[0021] Furthermore, in the step (3), the particle size of the granulated product is 96 μm to 900 μm, accounting for more than 90%, and the composition and particle strength meet the requirements of boiling chlorination.
[0022] Compared with the prior art, the beneficial technical effects of the present invention are:
[0023] (1) The composite binder for granulating fine-grained titanium-rich materials described in the present invention has a wide range of raw materials and low cost, and is applicable to existing fine-grained titanium-rich material granulation methods. At the same time, boiling chlorination dust collection residue is recycled to achieve solid waste recycling.
[0024] (2) The present invention provides a method for granulating fine-grained titanium-rich materials, which has a simple process and low requirements on equipment. The granulated products have good cold strength and hot strength, good stability in a high-temperature chlorination boiling furnace, high quality, and can meet the requirements of the boiling chlorination process. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] The composite binder of the present invention is alkali metal silicate and boiling chlorinated residue, the ratio of the two is 1-10:1, and the mixing mass ratio of the composite binder to the fine-grained titanium-rich material is 0.2-3wt%. When the binder addition amount is less than 0.2wt%, the binder has limited effect and the particle size of the granulated product is too small; when the binder addition amount is greater than 3wt%, too much binder makes the particle size of the fine-grained titanium-rich material granulated product too large.
[0027] In the present invention, the wear index of the product particles is measured by reducing the pulverization drum as a characterization method for the cold strength and hot strength of the product particles. The drum size is Φ130×200mm, the rotation speed is 30 rpm, and the time is 10 minutes. Each time, 100g of the dried or roasted granular material distributed in 96-900μm and cooled to room temperature is weighed for testing. Each test is repeated 3 times, and the arithmetic mean value is taken as the wear index RDI.
[0028]
[0029] Where: m 1 —The mass of the sample before drum rotation;
[0030] m 2 —Mass after drumming +96μm.
[0031] The calcination treatment method of the granular product is as follows: weigh 300g of dry particles with a particle size distribution of 96 to 900μm, place them in a Φ20×10cm graphite crucible by wrapping them up and down with coke powder (particle size greater than 5mm, washed until there are no fine powder particles on the surface and completely dried), and calcine them in a muffle furnace at 1000℃ for 60 minutes.
[0032] The above ideal embodiments of the present invention are for inspiration, and all other embodiments obtained by those skilled in the art without creative work belong to the protection scope of the present invention.
[0033] In the embodiment, the boiling chlorinated dust collecting residue comprises the following components, and the mass percentage of each component is:
[0034] Fe 5~11wt%; Al 1~3wt%; Ti5~9wt%; Mn 3~15wt%; Si 1~8wt%; Mg 1~5wt%; Ca 1~5wt%; C 30~50wt%; Cl 30~40wt%.
[0035] The main components of fine-grained artificial rutile and high-titanium slag raw materials used in the examples are shown in Table 1:
[0036] Table 1 Main chemical composition of fine-grained titanium-rich materials
[0037] Chemical composition / wt% <![CDATA[TiO 2 ]]> MgO CaO Fine-grained high-titanium slag 87.52 0.39 0.23 Fine-grained synthetic rutile 90.18 0.13 0.14
[0038] The effects of the composite adhesive of the present invention are described in conjunction with the following specific embodiments.
[0039] Example 1
[0040] Weigh 30g of binder (sodium silicate: boiling chlorinated dust collection residue = 5:1) and mix well with 1000g of fine-grained artificial rutile, place in a fluidized bed granulator, fluidize at a speed of 0.23m / s, and fill rate of material at 0.9%. Spray 300g of water through the atomizer of the fluidized bed granulator, disperse the binder liquid to the surface of the material, mix and condense into particles under the action of pneumatic, atomize at a pressure of 0.2MPa, and spray for 60min. The granulated product is dried and consolidated under the action of fluidized air, and the particle size distribution is 96μm-900μm, accounting for 90%, and TiO 2 The content of the product is 90.16%, and the content of CaO+MgO is 0.26%. The cold strength wear coefficient of the granular product is 8.84%, and the hot strength wear coefficient is 3.45%.
[0041] TiO in products 2 The content is 90.16%, and the content of CaO+MgO is 0.26%. The difference is very small compared with the main chemical components of the raw materials and can be ignored, which proves that the binder provided by the present invention does not affect the product grade. The cold strength wear coefficient of the product granules is 8.84%, and the hot strength wear coefficient is 3.45%, which proves that the obtained product has good cold strength and hot strength, and the hot strength is greater than the cold strength, indicating that the strength of the granules increases after high temperature treatment. It can be proved that the granulated product obtained by the binder provided by the present invention has good stability in a high-temperature chlorination boiling furnace and meets the requirements of the boiling chlorination process.
[0042] Example 2
[0043] Weigh 20g of binder (sodium silicate: boiling chlorinated dust collection residue = 10:1), 200g of water, and 1000g of fine-grained artificial rutile, mix them evenly, place them in a high-speed stirring granulation equipment, set the stirring blade speed to 400rpm, the cutting knife speed to 1000rpm, and the granulation time to 400s. The fine-grained artificial rutile is fully granulated. After drying, consolidation and screening, the granulated product has a particle size distribution of 96μm-900μm, accounting for 92%, and TiO 2The content of the product is 90.14%, the content of CaO+MgO is 0.25%. The cold strength wear coefficient of the granular product is 7.62%, and the hot strength wear coefficient is 3.34%.
[0044] TiO in products 2 The content is 90.14%, and the content of CaO+MgO is 0.25%. The difference is very small compared with the main chemical components in the raw material and can be ignored, which proves that the binder provided by the present invention does not affect the product grade. The cold strength wear coefficient of the product granules is 7.62%, and the hot strength wear coefficient is 3.34%, which proves that the obtained product has good cold strength and hot strength, and the hot strength is greater than the cold strength, indicating that the strength of the granules increases after high temperature treatment. It can be proved that the granulated product obtained by the binder provided by the present invention has good stability in a high-temperature chlorination boiling furnace and meets the requirements of the boiling chlorination process.
[0045] Example 3
[0046] Weigh 20g of binder (sodium silicate: boiling chlorinated dust collection residue = 3:1) and mix thoroughly with 1000g of fine-grained high-titanium slag, then put it into the feed hopper and evenly enter the rotating disc through the material distributor. Spray 200g of water evenly on the surface of the material through a spray gun for granulation. The disc diameter is 14 inches, the speed is 45r / min, the angle is 42°, and the granulation time is 15min. After drying the granulated product at 500℃ for several seconds, it is calcined at 900-1000℃ for 10-20min to obtain a particle size distribution of 96μm-900μm accounting for 90%, TiO 2 The content of the product is 87.50%, the content of CaO+MgO is 0.60%. The cold strength wear coefficient of the granular product is 8.48%, and the hot strength wear coefficient is 3.26%.
[0047] TiO in products 2 The content is 87.50%, and the CaO+MgO content is 0.60%, which is very different from that in the raw material and can be ignored, proving that the binder provided by the present invention does not affect the product grade. The cold strength wear coefficient of the product granules is 8.48%, and the hot strength wear coefficient is 3.26%, proving that the obtained product has good cold strength and hot strength, and the hot strength is greater than the cold strength, indicating that the particle strength increases after high temperature treatment, which can prove that the granulated product obtained by the binder provided by the present invention has good stability in a high-temperature chlorination boiling furnace and meets the requirements of the boiling chlorination process.
[0048] Example 4
[0049] Weigh 20g of binder (sodium silicate: boiling chlorinated dust collection residue = 1:1) and mix with 1000g of fine high-titanium slag and place in a V-type mixing granulator. Add 150g of water at a speed of 40r / min through the built-in stirring system of the mixer. After sufficient mixing, set the stirring rod speed to 1500-3000r / min. The granulation time is 96μm-900μm, accounting for 93%, and TiO 2 The content of the product is 87.51%, and the content of CaO+MgO is 0.63%. The cold strength wear coefficient of the granular product is 8.51%, and the hot strength wear coefficient is 3.28%.
[0050] TiO in products 2 The content is 87.51%, CaO+MgO content is 0.63%, which is equal to the TiO 2 The difference between the content of 90.18% and the content of CaO+MgO of 0.76% is very small and can be ignored, which proves that the binder provided by the present invention does not affect the product grade. The cold strength wear coefficient of the product granules is 8.51%, and the hot strength wear coefficient is 3.28%, which proves that the obtained product has good cold strength and hot strength, and the hot strength is greater than the cold strength, indicating that the strength of the granules increases after high temperature treatment. It can be proved that the granulated product obtained by the binder provided by the present invention has good stability in a high-temperature chlorination boiling furnace and meets the requirements of the boiling chlorination process.
[0051] Example 5
[0052] Weigh 20g of binder (potassium silicate: boiling chlorinated dust collection residue = 10:1), 200g of water, and 1000g of fine-grained artificial rutile, mix them evenly, place them in a high-speed stirring granulation equipment, set the stirring paddle speed to 400rpm, the cutting knife speed to 1000rpm, and the granulation time to 400s. The fine-grained artificial rutile is fully granulated. After drying, consolidation and screening, the granulated product has a particle size distribution of 96μm-900μm, accounting for 92%, and TiO 2 The product has a CaO+MgO content of 90.16% and a CaO+MgO content of 0.25%. The cold strength wear coefficient of the granular product is 8.58%, and the hot strength wear coefficient is 3.24%.
[0053] TiO in products 2 The content is 90.16%, and the content of CaO+MgO is 0.25%. The difference is very small compared with the main chemical components in the raw material and can be ignored, which proves that the binder provided by the present invention does not affect the product grade. The cold strength wear coefficient of the product granules is 8.58%, and the hot strength wear coefficient is 3.24%, which proves that the obtained product has good cold strength and hot strength, and the hot strength is greater than the cold strength, indicating that the strength of the granules increases after high temperature treatment. It can be proved that the granulated product obtained by the binder provided by the present invention has good stability in a high-temperature chlorination boiling furnace and meets the requirements of the boiling chlorination process.
[0054] Example 6
[0055] Weigh 2g of binder (sodium silicate: boiling chlorinated dust collection residue = 10:1), 100g of water, and 1000g of fine-grained high-titanium slag, mix them evenly, place them in a high-speed stirring granulation equipment, set the stirring blade speed to 300rpm, the cutting knife speed to 1000rpm, and the granulation time to 500s. The fine-grained high-titanium slag is fully granulated. After drying, consolidation and screening, the granulated product has a particle size distribution of 96μm-900μm, accounting for 87%, and TiO 2 The content of the product is 87.53%, the content of CaO+MgO is 0.62%. The cold strength wear coefficient of the granular product is 9.62%, and the hot strength wear coefficient is 5.14%.
[0056] TiO in products 2 The content is 87.53%, and the content of CaO+MgO is 0.62%. The difference is very small compared with the main chemical components in the raw material and can be ignored, which proves that the binder provided by the present invention does not affect the product grade. The cold strength wear coefficient of the product granules is 9.62%, and the hot strength wear coefficient is 5.14%, which proves that the obtained product has good cold strength and hot strength, and the hot strength is greater than the cold strength, indicating that the strength of the granules increases after high temperature treatment. It can be proved that the granulated product obtained by the binder provided by the present invention has good stability in a high-temperature chlorination boiling furnace and meets the requirements of the boiling chlorination process.
[0057] Comparative Example 1
[0058] Weigh 70g of binder (sodium silicate: boiling chlorinated dust collection residue = 10:1) and mix thoroughly with 1000g of fine-grained artificial rutile and place in a fluidized bed granulator. The fluidization speed is 0.23m / s and the material filling rate is 0.9%. 300g of water is sprayed through the atomizer of the fluidized bed granulator. The dispersed binder liquid is distributed to the surface of the material, mixed and condensed into particles under the action of pneumatics. The atomization pressure is 0.2MPa and the spraying time is 60min. The granulated product is dried and consolidated under the action of fluidized wind to obtain a product with a particle size distribution of 96μm to 900μm accounting for only 25%. Too much binder, the proportion of large particles increases, and the granulation effect is poor.
[0059] Comparative Example 2
[0060] 1000g of fine-grained artificial rutile was weighed and placed in a fluidized bed granulator, the fluidization speed was 0.24m / s, and the material filling rate was 0.9%. 300g of water was sprayed through the atomizer of the fluidized bed granulator, dispersed on the surface of the material, mixed and condensed into particles under the action of pneumatic motion, the atomization pressure was 0.2MPa, and the spraying time was 60min. The granulated product was dried and consolidated under the action of fluidized wind, and the particle size distribution was 96μm to 900μm, accounting for 10%. Without a binder, fine-grained artificial rutile is difficult to bond into agglomerates, and the granulation effect is poor.
[0061] Comparative Example 3
[0062] Weigh 30g of sodium silicate and 1000g of fine-grained high-titanium slag, mix thoroughly and place in a fluidized bed granulator, the fluidization speed is 0.23m / s, and the material filling rate is 0.9%. 300g of water is sprayed through the atomizer of the fluidized bed granulator, and the dispersed binder liquid is distributed to the surface of the material, mixed and condensed into particles under the action of pneumatics, the atomization pressure is 0.2MPa, and the spraying time is 60min. The granulated product is dried and consolidated under the action of fluidized wind, and the product with a particle size distribution of 96μm to 900μm accounts for only 36%
[0063] Comparative Example 4
[0064] Weigh 20g boiling chlorinated dust collection residue and 1000g fine-grained artificial rutile, mix them thoroughly and place them in a fluidized bed granulator. The fluidization speed is 0.23m / s and the material filling rate is 0.9%. 300g of water is sprayed through the atomizer of the fluidized bed granulator. The dispersed binder liquid is distributed to the surface of the material, mixed and condensed into particles under the action of pneumatics. The atomization pressure is 0.2MPa and the spraying time is 60min. The granulated product is dried and consolidated under the action of fluidized air to obtain a product with a particle size distribution of 96μm to 900μm accounting for only 10%.
[0065] In summary, the binder proposed in the present invention is suitable for various existing granulation methods for fine-grained titanium-rich materials, can make the product have good cold strength and hot strength, enhance the stability of the granulated product in a high-temperature chlorination boiling furnace, and has no effect on the product quality and the boiling chlorination furnace. In addition, the raw materials of this binder are extensive and the cost is low.
[0066] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and changes obtained without departing from the technical concept of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A composite binder for granulating fine titanium-rich materials, It is characterized in that The invention comprises silicate and boiling chlorinated dust collecting residue, wherein the mass ratio of the silicate to the boiling chlorinated dust collecting residue is 1 to 10:
1.
2. The composite binder for granulating fine titanium-rich materials according to claim 1, It is characterized in that The silicate is an alkali metal silicate.
3. The composite binder for granulating fine titanium-rich materials according to claim 1, It is characterized in that The boiling chlorinated dust collecting residue comprises the following components, and the mass percentage of each component is: Fe5-11wt%; Al 1~3wt%; Ti5~9wt%; Mn 3~15wt%; Si 1~8wt%; Mg 1~5wt%; Ca 1~5wt%; C 30~50wt%; Cl 30~40wt%.
4. A method for granulating fine titanium-rich materials, It is characterized in that The following steps are involved: (1) Preparation of composite adhesive: Weigh the adhesives according to a set ratio and mix them evenly to obtain a composite adhesive. (2) Mixing fine-grained titanium-rich materials: Fully mix the prepared composite binder with the fine-grained titanium-rich materials. Weigh a certain proportion of water and add it to the fine-grained titanium-rich materials that have been mixed evenly to fully mix the fine-grained titanium-rich materials, the composite binder and the water. (3) Granulation: The uniformly mixed fine-grained titanium-rich material granulation raw materials are placed into a granulation device, and the granulation product is obtained after drying.
5. A method for granulating fine titanium-rich material according to claim 4, It is characterized in that In the step (1), the added amount of the composite binder is 0.2 to 3 wt% of the mass of the fine-grained titanium-rich material.
6. A method for granulating fine titanium-rich material according to claim 4, It is characterized in that In the step (2), the fine-grained titanium-rich material refers to high-titanium slag, artificial rutile, or natural rutile with a particle size less than 96 μm.
7. A method for granulating fine titanium-rich material according to claim 4, It is characterized in that In the step (2), the amount of water added is 10 to 30 wt % of the mass of the fine-grained titanium-rich material.
8. A method for granulating fine titanium-rich material according to claim 4, It is characterized in that In the step (2), water is added to the raw materials in the form of a spray and mixed evenly.
9. A method for granulating fine titanium-rich material according to claim 4, It is characterized in that In the step (3), the granulation method of the fine titanium-rich material includes fluidized bed granulation method, disc granulation method, V-type mixer granulation method and high-speed stirring granulation method.
10. A method for granulating fine titanium-rich material according to claim 4, It is characterized in that In the step (3), the particle size of the granulated product is 96 μm to 900 μm, accounting for more than 90%, and the composition and particle strength meet the requirements of boiling chlorination.
Citation Information
Cited By
Granulation method of fine-fraction titanium-rich material
CN121629188A