Additive manufacturing titanium-molybdenum alloy and preparation method and application thereof
Through the additive manufacturing method combining aerosol powdering and laser selection melting and forming, the heat treatment is optimized, and the problems of high tissue uniformity and cost in the preparation of titanium alloys are solved, and high strength, low elastic modulus and biocompatibility are achieved. titanium-molybdenum alloy preparation meets the needs of the medical field.
Patent Information
- Application Number
- CN202411183521.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The existing titanium alloy preparation process has problems such as unstable tissue uniformity, complex processing process and high cost, which is difficult to meet the medical field's demand for high strength, low elastic modulus and biocompatibility.
Using an additive manufacturing method combining aerosol powdering and laser selection melting forming, titanium with high strength, low elastic modulus, good plasticity and formability, corrosion resistance and biocompatible through heat treatment optimization Molybdenum alloy.
The titanium-molybdenum alloy has achieved strong structural uniformity and good performance matching, simplified the process flow, reduced costs, and has a wider application prospect and personalized customization capabilities.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of alloy additive manufacturing, and relates to an additively manufactured titanium-molybdenum alloy and a preparation method and use thereof. Background Art
[0002] Titanium and titanium alloys are an important type of metal material. Due to their high specific strength, excellent heat resistance, and super corrosion resistance, they are widely used in aerospace, medical and other fields. In the medical field, titanium and titanium alloys have become the preferred raw materials for medical implants such as artificial joints, bone trauma products, spinal orthopedic internal fixation systems, dental implants, dental trays, dental orthopedic wires, artificial heart valves, and interventional cardiovascular stents due to their excellent properties such as high strength, non-magnetic, and biocompatibility. Due to the limited strength of titanium itself, the use of titanium alloys can improve the strength, but it is difficult to polish and has poor wear resistance, resulting in great processing difficulties, thus limiting its use in large load-bearing parts.
[0003] Titanium alloys include α-type titanium alloys and β-type titanium alloys. Alone α-type titanium alloys may still have the above problems, so the current focus is on the development of β-type titanium alloys and α+β-type titanium alloys. β-type titanium alloys have high strength and good formability, and have low elastic modulus and super corrosion resistance alone, so they are highly valued and have been developed. Ti15Mo alloy, as a typical β-type titanium alloy, has low elastic modulus, high strength, excellent fatigue resistance, good plasticity and formability, excellent corrosion resistance and biocompatibility. It has obvious application advantages in the medical field, but in actual applications, it is subject to many restrictions on material preparation and processing technology. At present, it is mostly made of deformed bars through mechanical processing, such as rolling and forging processes, but the alloy processing process is difficult to control and the process flow is complex, resulting in unstable alloy organization uniformity.
[0004] CN 107217221A discloses a method for preparing a high-uniform Ti-15Mo titanium alloy bar blank, which comprises: selecting a Ti-15Mo titanium alloy ingot with qualified composition, heating and heat preservation, performing blanking forging, and crushing the coarse cast grains; then heating and heat preservation the blank after blanking, and performing homogenization treatment; then heating and heat preservation again, performing upsetting forging, and further improving the uniformity of the material structure; finally heating and heat preservation the blank, and performing straight drawing and rounding forging, so as to obtain a high-uniform Ti-15Mo titanium alloy bar blank. The method homogenizes the alloy structure and refines the grains by alternating high-temperature homogenization and forging deformation, but it still belongs to the traditional method, the control of the processing process is relatively difficult, the preparation steps are more, the process is complicated, and the cost is high.
[0005] CN 111515381A discloses a high-strength and high-toughness titanium alloy powder for laser additive manufacturing and a preparation method thereof. The chemical composition of the titanium alloy powder includes Ti, Al, Mo, Sn, Zr, Cr, V, Fe and impurity elements N, H, and O. The element composition of the titanium alloy is relatively complex, and it is not an alloy type with two or three elements as the main components, and its crystal phase type is unclear; the preparation method includes: batching according to the required alloy components, mixing the alloy raw materials evenly and pressing them into electrodes, melting them into alloy ingots through vacuum consumable smelting, forging them into rods, and finally using a crucible-free induction melting gas atomization method to prepare titanium alloy powder for laser additive manufacturing. Although the method uses a melting and gas atomization method to prepare alloy powder, it does not disclose the process during additive manufacturing, and according to the different alloy compositions and application fields, the requirements for alloy properties are also different, and the corresponding selection of preparation processes will also be different.
[0006] CN 111945032A discloses a 3D printing fine-grained titanium alloy and a preparation method thereof, wherein the element composition of the titanium alloy includes 3-5% Al, 0.05-0.15% B, 0.3-0.6% C, and the balance is Ti and inevitable impurity elements; the method also includes vacuum melting after proportioning according to the element composition, preparing alloy powder by gas atomization, preparing alloy sample by selective laser melting after screening, and then heat treating to obtain fine-grained titanium alloy. The method improves the strength of the alloy by adjusting the content of boron and carbon elements, and is different from the type and composition of titanium-molybdenum alloy, and the application field is also different, and the corresponding process operation is also different.
[0007] In summary, for the selection of titanium-molybdenum alloy preparation process, it is necessary to control the composition of elements according to application requirements and adopt additive manufacturing technology to ensure that the various properties of the alloy are well matched and can be customized according to needs. Summary of the invention
[0008] In view of the problems existing in the prior art, the purpose of the present invention is to provide an additively manufactured titanium-molybdenum alloy and a preparation method and use thereof. The method quickly prepares titanium-molybdenum alloy parts through a process combining aerosol powder making and additive manufacturing, and then optimizes the heat treatment process to make the titanium-molybdenum alloy have a strong uniformity of organization, a high strength, a low elastic modulus, and good matching; the preparation process is simple and the cost is low.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a method for preparing a titanium-molybdenum alloy by additive manufacturing, the method comprising the following steps:
[0011] (1) preparing titanium-molybdenum alloy raw materials according to elemental composition, and then smelting them to obtain alloy rods;
[0012] (2) preparing pre-alloyed powder by gas atomization of the alloy rod obtained in step (1), and then sieving to obtain alloy powder;
[0013] (3) preparing alloy parts by laser selective melting of the alloy powder obtained in step (2);
[0014] (4) The alloy parts obtained in step (3) are subjected to solution treatment and aging treatment in sequence to obtain the additively manufactured titanium-molybdenum alloy.
[0015] In the present invention, for the preparation of β-type titanium alloy, titanium-molybdenum alloy is taken as an example. Based on the defects of traditional mechanical processing methods, the present invention adopts an additive manufacturing method, through the forming and atomization process of alloy rods, to prepare alloy powder of suitable particle size, and then adopts a laser selected melting method to accumulate layer by layer to quickly manufacture titanium-molybdenum alloy, and then through the optimization and adjustment of the heat treatment process, it is ensured that the uniformity of the alloy structure is strong, and it has high strength, low elastic modulus, good plasticity and formability, strong corrosion resistance, good biocompatibility, good matching of various properties, and can be customized according to application requirements; the method has a simple preparation process, low raw materials and costs, high material utilization rate, and has a wider application prospect.
[0016] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0017] As a preferred technical solution of the present invention, the titanium-molybdenum alloy in step (1) includes Ti15Mo alloy.
[0018] Preferably, the raw materials of the titanium-molybdenum alloy in step (1) include titanium and molybdenum.
[0019] Preferably, the titanium element includes TA1 and / or TA2, and the molybdenum element includes Mo1 molybdenum rod, and the Mo1 molybdenum rod is a high-purity molybdenum rod.
[0020] Preferably, the composition of the alloy bar in step (1) includes, by mass fraction: Mo 14.5-15.5%, such as 14.5%, 14.6%, 14.8%, 15%, 15.2%, 15.4% or 15.5%, etc., Fe≤0.1%, such as 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04% or 0.02%, etc., C 0.02-0.07%, such as 0.02%, 0.03%, 0.04%, 0.05%, 0.06% or 0.07%, etc., O 0.05-0.08%, for example, 0.05%, 0.055%, 0.06%, 0.065%, 0.07%, 0.075% or 0.08%, etc., the balance being Ti and other impurity elements; but not limited to the listed values, and other unlisted values within the respective numerical ranges are also applicable.
[0021] In the present invention, in addition to titanium and molybdenum as the main elements in the alloy rod raw material, the selection of the content of trace elements such as C and O has a significant impact on the preparation process of the alloy. Since titanium alloy has a high reaction activity to oxygen, oxygenation will occur during the laser selective melting forming process, and the oxygen content of the parts will be higher than that in the powder. Therefore, the oxygen content of the initial powder should not be too high. The C element content will affect the defects and microcracks in the forming process, so its content needs to be controlled.
[0022] Preferably, the other impurity elements include, by mass fraction: N≤0.03%, for example, 0.03%, 0.025%, 0.02%, 0.015% or 0.01%, etc., but are not limited to the listed values, and other values not listed within the numerical range are equally applicable; H≤0.0125%, for example, 0.0125%, 0.012%, 0.011%, 0.01%, 0.009%, 0.008%, 0.006% or 0.005%, etc., but are not limited to the listed values, and other values not listed within the numerical range are equally applicable.
[0023] As a preferred technical solution of the present invention, the smelting in step (1) is vacuum smelting, and the absolute pressure of the vacuum smelting is ≤0.2Pa, for example, 0.2Pa, 0.18Pa, 0.15Pa, 0.12Pa, 0.1Pa, 0.08Pa or 0.05Pa, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the smelting current of the smelting in step (1) is 5 to 12 kA, for example, 5 kA, 6 kA, 7 kA, 8 kA, 9 kA, 10 kA, 11 kA or 12 kA, but is not limited to the listed values, and other values not listed in the numerical range are also applicable; the smelting voltage is 30 to 40 V, for example, 30 V, 31 V, 32 V, 33 V, 34 V, 35 V, 36 V, 37 V, 38 V, 39 V or 40 V, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0025] Preferably, the smelting speed in step (1) is 2 to 10 kg / min, for example, 2 kg / min, 3 kg / min, 4 kg / min, 5 kg / min, 6 kg / min, 7 kg / min, 8 kg / min, 9 kg / min or 10 kg / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] Preferably, the alloy rod is formed after the smelting in step (1) by placing it in a mold and cooling it.
[0027] Preferably, the diameter of the alloy rod in step (1) is 40 to 50 mm, for example, 40 mm, 42 mm, 44 mm, 45 mm, 46 mm, 48 mm or 50 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] As a preferred technical solution of the present invention, the gas atomization method in step (2) comprises: firstly melting the alloy rod, then spraying it into mist using gas, and then condensing it to form pre-alloyed powder.
[0029] Preferably, the aerosolization method in step (2) is carried out using vacuum induction aerosolization powder making equipment, and the vacuum induction aerosolization powder making equipment is provided with an induction coil.
[0030] Preferably, when the alloy rod is melted, the power of the induction coil is 24-32 kW, for example, 24 kW, 25 kW, 27 kW, 28 kW, 30 kW or 32 kW, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the feed speed of the alloy rod is 40-55 mm / min, for example, 40 mm / min, 42 mm / min, 45 mm / min, 48 mm / min, 50 mm / min, 52 mm / min or 55 mm / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the gas injection uses an inert gas, which includes helium, neon or argon, and the pressure of the gas injection is 35-42 mbar, for example, 35 mbar, 36 mbar, 37 mbar, 38 mbar, 39 mbar, 40 mbar, 41 mbar or 42 mbar, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable. The pressure is an absolute pressure, and the environment is still a vacuum under these numerical conditions.
[0033] Preferably, the pre-alloyed powder in step (2) is screened by airflow screening and vibration screening.
[0034] Preferably, the particle size range of the alloy powder in step (2) is 10 to 53 μm, for example, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm or 53 μm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] In the present invention, the airflow screening and vibration screening are used successively. The airflow screening mainly screens the lower limit of the powder particle size and blows and separates the powder with smaller particle size. The vibration screening mainly screens the upper limit of the powder particle size and intercepts the particles with too large particle size, so as to obtain alloy powder with a suitable particle size range.
[0036] As a preferred technical solution of the present invention, the laser selective melting forming method described in step (3) is a 3D printing forming method. Before the operation, process data is prepared according to the design drawings of the alloy parts to be prepared to generate engineering files.
[0037] Preferably, the laser selective melting forming in step (3) is carried out using a laser selective melting forming device, wherein a forming chamber is provided, a substrate is provided in the forming chamber, and alloy powder is laid on the substrate.
[0038] Preferably, the alloy powder is firstly baked and kept warm before being loaded into the forming chamber.
[0039] Preferably, the baking temperature is 80-120°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C, but is not limited to the listed values, and other values not listed within the numerical range are equally applicable; the insulation time is 2-8h, for example, 2h, 3h, 4h, 5h, 6h, 7h or 8h, but is not limited to the listed values, and other values not listed within the numerical range are equally applicable.
[0040] Preferably, the substrate in the forming chamber is preheated first, and the preheating temperature of the substrate is 25-200°C, for example, 25°C, 40°C, 60°C, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C or 200°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] Preferably, the powder thickness on the substrate is 0.02-0.04 mm, for example, 0.02 mm, 0.022 mm, 0.025 mm, 0.027 mm, 0.03 mm, 0.032 mm, 0.035 mm, 0.038 mm or 0.04 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] As a preferred technical solution of the present invention, in the laser selective melting forming process of step (3), the alloy powder is melted by laser, and after sintering and solidification, the powder is repeatedly spread and stacked layer by layer to form an alloy part.
[0043] Preferably, during the laser selective melting forming process in step (3), an inert gas is introduced into the forming chamber, and the inert gas includes helium, neon or argon, etc., and the oxygen content is controlled to be below 1000 ppm, for example, 1000 ppm, 900 ppm, 800 ppm, 700 ppm, 600 ppm, 600 ppm, 400 ppm or 300 ppm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] Preferably, during the laser selective melting forming in step (3), the laser power is 170-265 W, for example, 170 W, 180 W, 200 W, 210 W, 220 W, 230 W, 240 W, 250 W, 260 W or 265 W, etc., the spot diameter is 0.02-0.2 mm, for example, 0.02 mm, 0.05 mm, 0.08 mm, 0.1 mm, 0.12 mm, 0.15 mm, 0.18 mm or 0.2 mm, etc., and the scanning speed is 700-1400 mm / s, for example, 700 mm / s, 800 mm / s, 900 mm / s, 1000 mm / s, 1100 mm / s, 1200 mm / s, 1300 mm / s or 1400 mm / s, etc.; but it is not limited to the listed values, and other values not listed within the respective numerical ranges are also applicable.
[0045] Preferably, after the alloy part is formed in step (3), the alloy part is taken out after the substrate temperature drops below 70°C, for example, 70°C, 65°C, 60°C, 55°C, 50°C, 45°C, 40°C, 35°C or 30°C, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0046] As a preferred technical solution of the present invention, the temperature of the solution treatment in step (4) is 750-850°C, for example, 750°C, 760°C, 780°C, 800°C, 820°C, 840°C or 850°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] Preferably, the holding time of the solution treatment in step (4) is 0.5 to 2 h, for example 0.5 h, 0.75 h, 1 h, 1.25 h, 1.5 h, 1.75 h or 2 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0048] Preferably, the alloy part after the solution treatment is cooled in an inert gas, and the inert gas includes helium, neon or argon.
[0049] Preferably, the temperature of the aging treatment in step (4) is 450-580°C, for example, 450°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C or 580°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0050] Preferably, the holding time of the aging treatment in step (4) is 0.5 to 2 h, for example, 0.5 h, 0.75 h, 1 h, 1.25 h, 1.5 h, 1.75 h or 2 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0051] In the present invention, the solution treatment and aging treatment are both carried out in a vacuum heat treatment furnace, and the pressure in the furnace during heat treatment is below 0.1 Pa, for example, 0.1 Pa, 0.08 Pa, 0.06 Pa, 0.05 Pa, 0.04 Pa, 0.02 Pa or 0.01 Pa, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0052] Preferably, the alloy parts after the solution treatment and the aging treatment are cooled in an inert gas. The temperature can be directly lowered from the solution treatment temperature to the aging treatment temperature for insulation, or it can be first lowered to room temperature and then heated again for aging treatment; the inert gas includes helium, neon or argon.
[0053] In the present invention, the main function of the solid solution and aging heat treatment is to eliminate the residual stress inside the alloy parts prepared by the laser selective melting method, thereby improving the mechanical properties thereof.
[0054] As a preferred technical solution of the present invention, after step (4) is completed, the support structure on the alloy part is removed, and the support structure refers to an additional temporary structure added to the part model to prevent some suspended parts in the part from collapsing during the printing process.
[0055] Preferably, the support structure is removed by manual removal or mechanical removal.
[0056] Preferably, after removing the support structure, polishing, sandblasting, cleaning and drying are performed in sequence to obtain the additively manufactured titanium-molybdenum alloy.
[0057] Preferably, the polishing includes vibration polishing, and the roughness of the part surface after polishing reaches below 6.3μm, for example 6.3μm, 6μm, 5.5μm, 5μm, 4.5μm, 4μm or 3μm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0058] Preferably, the roughness of the part surface after sandblasting and polishing reaches below 3.2 μm, for example 3.2 μm, 3 μm, 2.5 μm, 2 μm, 1.5 μm or 1 μm, etc., but is not limited to the listed values. Other unlisted values within the numerical range are also applicable. At this time, the appearance quality of the parts is more uniform.
[0059] Preferably, the cleaning is ultrasonic cleaning using an organic solvent.
[0060] Preferably, the organic solvent comprises ethanol and / or acetone.
[0061] Preferably, the drying comprises vacuum drying, the drying temperature is 80-120°C, for example 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C, and the time is 1-4h, for example 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0062] In a second aspect, the present invention provides an additively manufactured titanium-molybdenum alloy obtained by the above-mentioned preparation method, wherein the titanium-molybdenum alloy includes a Ti15Mo alloy.
[0063] Preferably, the composition of the titanium-molybdenum alloy includes, by mass fraction: Mo 14.5-15.5%, such as 14.5%, 14.6%, 14.8%, 15%, 15.2%, 15.4% or 15.5%, etc., Fe≤0.1%, such as 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04% or 0.02%, etc., C 0.02-0.07%, such as 0.02%, 0.03%, 0.04%, 0.05%, 0.06% or 0.07%, etc., O 0.07-0.1%, for example, 0.07%, 0.075%, 0.08%, 0.085%, 0.09%, 0.095% or 0.1%, etc., the remainder being Ti and other impurity elements; but not limited to the listed values, and other unlisted values within the respective numerical ranges are also applicable.
[0064] In a third aspect, the present invention provides a use of the above-mentioned additively manufactured titanium-molybdenum alloy, wherein the additively manufactured titanium-molybdenum alloy is used as a biomedical material, preferably as a medical implant.
[0065] Compared with the prior art, the present invention has the following beneficial effects:
[0066] (1) The method of the present invention prepares alloy powder of suitable particle size through the forming and atomization process of alloy rods, and then uses the laser selective melting method to accumulate layer by layer to quickly manufacture titanium-molybdenum alloy, and then optimizes and adjusts the heat treatment process to ensure that the alloy structure is highly uniform, has high strength, low elastic modulus, good plasticity and formability, strong corrosion resistance, good biocompatibility, and good matching of various properties;
[0067] (2) The titanium-molybdenum alloy prepared by the method of the present invention can be customized according to application requirements and actual patient conditions;
[0068] (3) The method of the present invention has a simple preparation process, low raw material and process costs, high material utilization rate, and has a wider application prospect. DETAILED DESCRIPTION
[0069] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0070] The specific implementation method of the present invention provides a method for preparing a titanium-molybdenum alloy by additive manufacturing, and the preparation method comprises the following steps:
[0071] (1) preparing titanium-molybdenum alloy raw materials according to elemental composition, and then smelting them to obtain alloy rods;
[0072] (2) preparing pre-alloyed powder by gas atomization of the alloy rod obtained in step (1), and then sieving to obtain alloy powder;
[0073] (3) preparing alloy parts by laser selective melting of the alloy powder obtained in step (2);
[0074] (4) The alloy parts obtained in step (3) are subjected to solution treatment and aging treatment in sequence to obtain the additively manufactured titanium-molybdenum alloy.
[0075] The following are typical but non-limiting embodiments of the present invention:
[0076] Embodiment 1:
[0077] This embodiment provides a method for preparing a titanium-molybdenum alloy by additive manufacturing, the method comprising the following steps:
[0078] (1) titanium and molybdenum are mixed according to the elemental composition, and then vacuum smelted. The vacuum smelting current is 8 kA, the voltage is 36 V, the absolute pressure is 0.15 Pa, and the smelting speed is 6 kg / min. After smelting, the alloy rod is placed in a mold for cooling to obtain an alloy rod. The alloy rod has a diameter of 45 mm. The composition of the alloy rod includes, by mass fraction, Mo 15.0%, Fe 0.08%, C 0.05%, O 0.06%, N 0.03%, H 0.0125%, and the balance is Ti;
[0079] (2) The alloy rod obtained in step (1) is subjected to a gas atomization method to prepare a pre-alloyed powder, wherein the gas atomization method is carried out using a vacuum induction gas atomization powder making device, wherein the alloy rod is first melted, the power of the induction coil during melting is 28 kW, the feed speed of the alloy rod is 48 mm / min, and then argon gas is sprayed into a mist, the gas spray pressure is 40 mbar, and the pre-alloyed powder is formed by condensation, and then screened by airflow screening and vibration screening to obtain an alloy powder, wherein the particle size range of the alloy powder is 20 to 40 μm;
[0080] (3) preparing alloy parts by laser selective melting of the alloy powder obtained in step (2), wherein the process data is prepared according to the design drawings of the alloy parts to be prepared and an engineering file is generated before the operation; the alloy powder is first baked and kept warm at a temperature of 100° C. for 5 hours;
[0081] The laser selective melting forming is carried out by using a laser selective melting forming equipment, wherein a forming chamber is provided, wherein a substrate is provided in the forming chamber, and the substrate is preheated at 120° C.; alloy powder is spread on the substrate, and the thickness of the powder is 0.03 mm. During the laser selective melting forming process, argon gas is introduced into the forming chamber, and the oxygen content is controlled to be 800 ppm. The alloy powder is melted by laser, and the laser power is 220 W, the spot diameter is 0.1 mm, and the scanning speed is 1000 mm / s. After sintering and solidification, the powder is repeatedly spread, and the alloy parts are stacked layer by layer. After the alloy parts are formed, the temperature of the substrate drops to 70° C. and then the alloy parts are taken out;
[0082] (4) The alloy parts obtained in step (3) are subjected to solution treatment and aging treatment in sequence, wherein the temperature of the solution treatment is 800°C, the holding time is 1 hour, and the temperature is reduced in argon gas; the temperature of the aging treatment is 520°C, the holding time is 1 hour, and the temperature is reduced in argon gas; then the supporting structure on the alloy parts is removed by mechanical processing, and polishing, sandblasting, cleaning and drying are performed in sequence, wherein the polishing is vibration polishing, and the surface roughness of the parts after polishing reaches 6.0 μm, and the surface roughness after sandblasting is 2.8 μm, and ethanol is used for ultrasonic cleaning, and the drying temperature is 100°C and the time is 2.5 hours to obtain additively manufactured titanium-molybdenum alloy.
[0083] In this embodiment, the additively manufactured titanium-molybdenum alloy prepared by the above method has a tensile strength of 865 MPa, a yield strength of 780 MPa, an elongation of 24%, a compressive elastic modulus of 50 GPa, excellent mechanical properties, and good biocompatibility, and can be customized when used as an implant.
[0084] Embodiment 2:
[0085] This embodiment provides a method for preparing a titanium-molybdenum alloy by additive manufacturing, the method comprising the following steps:
[0086] (1) titanium and molybdenum are mixed according to the elemental composition, and then vacuum smelted. The vacuum smelting current is 10 kA, the voltage is 34 V, the absolute pressure is 0.18 Pa, and the smelting speed is 4 kg / min. After smelting, the alloy rod is placed in a mold for cooling to obtain an alloy rod. The alloy rod has a diameter of 40 mm. The composition of the alloy rod includes, by mass fraction, 14.5% Mo, 0.1% Fe, 0.07% C, 0.08% O, 0.02% N, 0.01% H, and the balance is Ti.
[0087] (2) The alloy rod obtained in step (1) is subjected to a gas atomization method to prepare a pre-alloyed powder, wherein the gas atomization method is carried out using a vacuum induction gas atomization powder making device, wherein the alloy rod is first melted, the power of the induction coil during melting is 24 kW, the feed speed of the alloy rod is 40 mm / min, and then argon gas is sprayed into a mist, the gas spray pressure is 42 mbar, and the pre-alloyed powder is formed by condensation, and then screened by airflow screening and vibration screening to obtain an alloy powder, wherein the particle size range of the alloy powder is 10 to 25 μm;
[0088] (3) preparing alloy parts by laser selective melting of the alloy powder obtained in step (2), wherein the process data is prepared according to the design drawings of the alloy parts to be prepared and an engineering file is generated before the operation; the alloy powder is first baked and kept warm at a temperature of 80° C. for 8 hours;
[0089] The laser selective melting forming is carried out by using a laser selective melting forming equipment, wherein a forming chamber is provided, wherein a substrate is provided in the forming chamber, and the substrate is preheated at 80° C.; alloy powder is spread on the substrate, and the thickness of the powder is 0.02 mm. During the laser selective melting forming process, argon gas is introduced into the forming chamber, and the oxygen content is controlled to be 600 ppm. The alloy powder is melted by laser, and the laser power is 170 W, the spot diameter is 0.05 mm, and the scanning speed is 700 mm / s. After sintering and solidification, the powder is repeatedly spread, and the alloy parts are stacked layer by layer. After the alloy parts are formed, the temperature of the substrate drops to 60° C. and then the alloy parts are taken out;
[0090] (4) The alloy parts obtained in step (3) are subjected to solution treatment and aging treatment in sequence, wherein the temperature of the solution treatment is 750°C, the holding time is 2 hours, and the temperature is reduced in argon gas; the temperature of the aging treatment is 450°C, the holding time is 2 hours, and the temperature is reduced in argon gas; then the supporting structure on the alloy parts is removed by mechanical processing, and polishing, sandblasting, cleaning and drying are performed in sequence, wherein the polishing is vibration polishing, and the surface roughness of the parts after polishing reaches 5.5 μm, and the surface roughness after sandblasting is 2.5 μm, and acetone is used for ultrasonic cleaning, and the drying temperature is 120°C and the time is 1 hour to obtain additively manufactured titanium-molybdenum alloy.
[0091] In this embodiment, the additively manufactured titanium-molybdenum alloy prepared by the above method has a tensile strength of 850 MPa, a yield strength of 765 MPa, an elongation of 28%, a compressive elastic modulus of 48 GPa, excellent mechanical properties, and good biocompatibility, and can be customized when used as an implant.
[0092] Embodiment 3:
[0093] This embodiment provides a method for preparing a titanium-molybdenum alloy by additive manufacturing, the method comprising the following steps:
[0094] (1) titanium and molybdenum are mixed according to the elemental composition, and then vacuum smelted. The vacuum smelting current is 6 kA, the voltage is 38 V, the absolute pressure is 0.12 Pa, and the smelting speed is 8 kg / min. After smelting, the alloy rod is placed in a mold for cooling to obtain an alloy rod. The alloy rod has a diameter of 50 mm. The composition of the alloy rod includes, by mass fraction, 15.5% Mo, 0.09% Fe, 0.02% C, 0.05% O, 0.025% N, 0.012% H, and the balance is Ti.
[0095] (2) The alloy rod obtained in step (1) is subjected to a gas atomization method to prepare a pre-alloyed powder, wherein the gas atomization method is carried out using a vacuum induction gas atomization powder making device, wherein the alloy rod is first melted, the power of the induction coil during melting is 32 kW, the feed speed of the alloy rod is 55 mm / min, and then argon gas is sprayed into a mist, the gas spray pressure is 35 mbar, and the pre-alloyed powder is formed by condensation, and then screened by airflow screening and vibration screening to obtain an alloy powder, wherein the particle size range of the alloy powder is 30 to 53 μm;
[0096] (3) preparing alloy parts by laser selective melting of the alloy powder obtained in step (2), wherein the process data is prepared according to the design drawings of the alloy parts to be prepared and an engineering file is generated before the operation; the alloy powder is first baked and kept warm at a temperature of 120° C. for 2 hours;
[0097] The laser selective melting forming is carried out by using a laser selective melting forming equipment, wherein a forming chamber is provided, wherein a substrate is provided in the forming chamber, and the substrate is preheated at 150° C.; alloy powder is spread on the substrate, and the thickness of the powder is 0.04 mm. During the laser selective melting forming process, argon gas is introduced into the forming chamber, and the oxygen content is controlled to be 1000 ppm. The alloy powder is melted by laser, and the laser power is 260 W, the spot diameter is 0.2 mm, and the scanning speed is 1400 mm / s. After sintering and solidification, the powder is repeatedly spread, and the alloy parts are stacked layer by layer. After the alloy parts are formed, the temperature of the substrate drops to 65° C. and then the alloy parts are taken out;
[0098] (4) The alloy parts obtained in step (3) are subjected to solution treatment and aging treatment in sequence, wherein the temperature of the solution treatment is 850°C, the holding time is 0.5h, and the temperature is reduced in argon gas; the temperature of the aging treatment is 580°C, the holding time is 0.5h, and the temperature is reduced in argon gas; then the support structure on the alloy parts is manually removed, and polishing, sandblasting, cleaning and drying are performed in sequence, wherein the polishing is vibration polishing, and the surface roughness of the parts after polishing reaches 5.0μm, and the surface roughness after sandblasting is 2.1μm, and ethanol is used for ultrasonic cleaning, and the drying temperature is 80°C and the time is 4h to obtain additively manufactured titanium-molybdenum alloy.
[0099] In this embodiment, the additively manufactured titanium-molybdenum alloy prepared by the above method has a tensile strength of 840 MPa, a yield strength of 760 MPa, an elongation of 29%, a compressive elastic modulus of 45 GPa, excellent mechanical properties, and good biocompatibility, and can be customized when used as an implant.
[0100] Embodiment 4:
[0101] This embodiment provides a method for preparing a titanium-molybdenum alloy by additive manufacturing, the method comprising the following steps:
[0102] (1) titanium and molybdenum are mixed according to the elemental composition, and then vacuum smelted. The vacuum smelting current is 12 kA, the voltage is 30 V, the absolute pressure is 0.16 Pa, and the smelting speed is 10 kg / min. After smelting, the alloy rod is placed in a mold for cooling to obtain an alloy rod. The alloy rod has a diameter of 42 mm. The composition of the alloy rod includes, by mass fraction, 15.2% Mo, 0.07% Fe, 0.04% C, 0.07% O, 0.03% N, 0.011% H, and the balance is Ti;
[0103] (2) The alloy rod obtained in step (1) is subjected to a gas atomization method to prepare a pre-alloyed powder, wherein the gas atomization method is carried out using a vacuum induction gas atomization powder making device, wherein the alloy rod is first melted, the power of the induction coil during melting is 26 kW, the feed speed of the alloy rod is 45 mm / min, and then neon gas is sprayed into a mist, the gas spray pressure is 38 mbar, and the pre-alloyed powder is formed by condensation, and then screened by airflow screening and vibration screening to obtain an alloy powder, wherein the particle size range of the alloy powder is 25 to 45 μm;
[0104] (3) preparing alloy parts by laser selective melting of the alloy powder obtained in step (2), wherein the process data is prepared according to the design drawings of the alloy parts to be prepared and an engineering file is generated before the operation; the alloy powder is first baked and kept warm at a temperature of 110° C. for 4 hours;
[0105] The laser selective melting forming is carried out by using a laser selective melting forming equipment, wherein a forming chamber is provided, wherein a substrate is provided in the forming chamber, and the substrate is preheated at 160° C.; alloy powder is spread on the substrate, and the thickness of the powder is 0.035 mm. During the laser selective melting forming process, neon gas is introduced into the forming chamber, and the oxygen content is controlled to be 900 ppm. The alloy powder is melted by laser, and the laser power is 200 W, the spot diameter is 0.15 mm, and the scanning speed is 800 mm / s. After sintering and solidification, the powder is repeatedly spread, and the alloy parts are stacked layer by layer. After the alloy parts are formed, the temperature of the substrate drops to 70° C. and then the alloy parts are taken out;
[0106] (4) The alloy parts obtained in step (3) are subjected to solution treatment and aging treatment in sequence, wherein the temperature of the solution treatment is 780°C, the holding time is 1.5 hours, and the parts are cooled in neon gas; the temperature of the aging treatment is 550°C, the holding time is 0.75 hours, and the parts are cooled in neon gas; then, the supporting structure on the alloy parts is manually removed, and polishing, sandblasting, cleaning and drying are performed in sequence, wherein the polishing is vibration polishing, and the surface roughness of the parts after polishing reaches 6.3 μm, and the surface roughness after sandblasting is 3.0 μm, and acetone is used for ultrasonic cleaning, and the drying temperature is 90°C and the time is 3 hours to obtain additively manufactured titanium-molybdenum alloy.
[0107] In this embodiment, the additively manufactured titanium-molybdenum alloy prepared by the above method has a tensile strength of 860 MPa, a yield strength of 775 MPa, an elongation of 25%, a compressive elastic modulus of 48 GPa, excellent mechanical properties, and good biocompatibility, and can be customized when used as an implant.
[0108] Embodiment 5:
[0109] This embodiment provides a method for preparing a titanium-molybdenum alloy by additive manufacturing, the method comprising the following steps:
[0110] (1) titanium and molybdenum are mixed according to the elemental composition, and then vacuum smelted. The vacuum smelting current is 7 kA, the voltage is 40 V, the absolute pressure is 0.14 Pa, and the smelting speed is 3 kg / min. After smelting, the alloy rod is placed in a mold for cooling to obtain an alloy rod. The alloy rod has a diameter of 48 mm. The composition of the alloy rod includes, by mass fraction, Mo 14.8%, Fe 0.06%, C 0.06%, O 0.06%, N 0.025%, H 0.012%, and the balance is Ti;
[0111] (2) The alloy rod obtained in step (1) is subjected to a gas atomization method to prepare a pre-alloyed powder, wherein the gas atomization method is carried out using a vacuum induction gas atomization powder making device, wherein the alloy rod is first melted, the power of the induction coil during melting is 30 kW, the feed speed of the alloy rod is 48 mm / min, and then neon gas is sprayed into a mist, the gas spray pressure is 36 mbar, and the pre-alloyed powder is formed by condensation, and then screened by airflow screening and vibration screening to obtain an alloy powder, wherein the particle size range of the alloy powder is 15 to 32 μm;
[0112] (3) preparing alloy parts by laser selective melting of the alloy powder obtained in step (2), wherein the process data is prepared according to the design drawings of the alloy parts to be prepared and an engineering file is generated before the operation; the alloy powder is first baked and kept warm at a temperature of 90° C. for 6 hours;
[0113] The laser selective melting forming is carried out by using a laser selective melting forming equipment, wherein a forming chamber is provided, wherein a substrate is provided in the forming chamber, and the substrate is preheated at 110° C.; alloy powder is spread on the substrate, and the thickness of the powder is 0.025 mm; during the laser selective melting forming process, neon gas is introduced into the forming chamber, and the oxygen content is controlled to be 850ppm; the alloy powder is melted by laser, and the laser power is 240W, the spot diameter is 0.08mm, and the scanning speed is 1200mm / s; after sintering and solidification, the powder is repeatedly spread, and the alloy parts are stacked layer by layer; after the alloy parts are formed, the temperature of the substrate drops to 55° C. and then the alloy parts are taken out;
[0114] (4) The alloy parts obtained in step (3) are subjected to solution treatment and aging treatment in sequence, wherein the temperature of the solution treatment is 820° C., the holding time is 0.75 h, and the parts are cooled in neon gas; the temperature of the aging treatment is 480° C., the holding time is 1.5 h, and the parts are cooled in neon gas; then, the supporting structure on the alloy parts is removed by mechanical processing, and polishing, sandblasting, cleaning and drying are performed in sequence, wherein the polishing is vibration polishing, and the surface roughness of the parts after polishing reaches 5.8 μm, and the surface roughness after sandblasting is 2.5 μm, and acetone is used for ultrasonic cleaning, and the drying temperature is 110° C. and the time is 2 h to obtain an additively manufactured titanium-molybdenum alloy.
[0115] In this embodiment, the additively manufactured titanium-molybdenum alloy prepared by the above method has a tensile strength of 855 MPa, a yield strength of 770 MPa, an elongation of 26%, a compressive elastic modulus of 46 GPa, excellent mechanical properties, and good biocompatibility, and can be customized when used as an implant.
[0116] Embodiment 6:
[0117] This embodiment provides a method for preparing titanium-molybdenum alloy by additive manufacturing. The preparation method refers to the method in Example 1, with the only difference being that the oxygen content of the alloy rod in step (1) is 0.1%.
[0118] In this embodiment, the oxygen content in the rod raw material is relatively high. When the titanium-molybdenum alloy is prepared by the above method, due to the high chemical reaction activity of the titanium-molybdenum alloy to oxygen, the tensile strength and yield strength of the material are increased, the tensile strength can reach 890MPa, the yield strength can reach 800MPa, the elongation is significantly reduced to 13%, and the compressive elastic modulus is 55GPa.
[0119] Embodiment 7:
[0120] This embodiment provides a method for preparing titanium-molybdenum alloy by additive manufacturing. The preparation method refers to the method in Example 1, with the only difference being that the carbon content of the alloy rod in step (1) is 0.1%.
[0121] In this embodiment, the carbon content in the rod raw material is relatively high. When the titanium-molybdenum alloy is prepared by the above method, since the carbon element will affect the material's control over defects and cracks, the tensile strength and yield strength of the material remain basically unchanged, the tensile strength is 860 MPa, the yield strength is 780 MPa, the elongation is reduced to 16%, and the compressive elastic modulus is 48 GPa.
[0122] From the above embodiments, it can be seen that the method of the present invention prepares alloy powder of suitable particle size through the forming and atomization process of alloy rods, and then adopts the laser selection melting method to accumulate layer by layer to quickly manufacture titanium-molybdenum alloy, and then optimizes and adjusts the heat treatment process to ensure that the alloy structure has strong uniformity, high strength, low elastic modulus, good plasticity and formability, strong corrosion resistance, good biocompatibility, and good matching of various properties; the titanium-molybdenum alloy prepared by the method can be personalized according to application requirements and actual patient conditions; the method has a simple preparation process, low raw material and process costs, high material utilization, and has a wider application prospect.
[0123] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the method of the present invention, addition of auxiliary operations, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing titanium-molybdenum alloy by additive manufacturing, characterized in that: The preparation method comprises the following steps: (1) preparing titanium-molybdenum alloy raw materials according to elemental composition, and then smelting them to obtain alloy rods; (2) preparing pre-alloyed powder by gas atomization of the alloy rod obtained in step (1), and then sieving to obtain alloy powder; (3) preparing alloy parts by laser selective melting of the alloy powder obtained in step (2); (4) The alloy parts obtained in step (3) are subjected to solution treatment and aging treatment in sequence to obtain the additively manufactured titanium-molybdenum alloy.
2. The preparation method according to claim 1, characterized in that: The titanium-molybdenum alloy in step (1) includes Ti15Mo alloy; Preferably, the raw materials of the titanium-molybdenum alloy in step (1) include titanium and molybdenum; Preferably, the titanium element includes TA1 and / or TA2, and the molybdenum element includes Mo1 molybdenum rod. Preferably, the composition of the alloy bar in step (1) includes, by mass fraction: Mo 14.5-15.5%, Fe≤0.1%, C 0.02-0.07%, O 0.05-0.08%, and the remainder is Ti and other impurity elements; Preferably, the other impurity elements include, by mass fraction: N≤0.03%, H≤0.0125%.
3. The preparation method according to claim 1 or 2, characterized in that: The smelting in step (1) is vacuum smelting, and the absolute pressure of the vacuum smelting is ≤0.2Pa; Preferably, the smelting current of the smelting in step (1) is 5 to 12 kA, and the smelting voltage is 30 to 40 V; Preferably, the smelting speed in step (1) is 2 to 10 kg / min; Preferably, the smelting in step (1) is placed in a mold and cooled to form an alloy rod; Preferably, the diameter of the alloy rod in step (1) is 40 to 50 mm.
4. The preparation method according to any one of claims 1 to 3, characterized in that The gas atomization method in step (2) comprises: firstly melting the alloy rod, then spraying it into a mist by gas, and then condensing it to form a pre-alloyed powder; Preferably, the aerosolization method in step (2) is carried out using a vacuum induction aerosolization powder making device, wherein the vacuum induction aerosolization powder making device is provided with an induction coil; Preferably, when the alloy rod is melted, the power of the induction coil is 24-32 kW; Preferably, the feeding speed of the alloy bar is 40-55 mm / min; Preferably, the gas injection uses an inert gas, and the pressure of the gas injection is 35-42 mbar; Preferably, the pre-alloyed powder in step (2) is screened by airflow screening and vibration screening; Preferably, the particle size of the alloy powder in step (2) is in the range of 10 to 53 μm.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The laser selective melting forming method in step (3) is a 3D printing forming method. Before the operation, process data is prepared according to the design drawings of the alloy parts to be prepared to generate engineering files; Preferably, the laser selective melting forming in step (3) is performed using a laser selective melting forming device, wherein a forming chamber is provided, a substrate is provided in the forming chamber, and alloy powder is laid on the substrate; Preferably, before the alloy powder is loaded into the forming chamber, the alloy powder is firstly baked and kept warm; Preferably, the baking temperature is 80-120°C and the insulation time is 2-8h; Preferably, the substrate in the forming chamber is preheated first, and the preheating temperature of the substrate is 25-200° C.; Preferably, the powder coating thickness on the substrate is 0.02-0.04 mm.
6. The preparation method according to any one of claims 1 to 5, characterized in that: In the laser selective melting forming process of step (3), the alloy powder is melted by laser, and after sintering and solidification, the powder is repeatedly spread and stacked layer by layer to form an alloy part; Preferably, during the laser selective melting forming process in step (3), an inert gas is introduced into the forming chamber to control the oxygen content to be below 1000 ppm; Preferably, during the laser selective melting in step (3), the laser power is 170-265 W, the spot diameter is 0.02-0.2 mm, and the scanning speed is 700-1400 mm / s; Preferably, after the alloy part is formed in step (3), the alloy part is taken out after the substrate temperature drops below 70°C.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The temperature of the solution treatment in step (4) is 750-850°C; Preferably, the holding time of the solution treatment in step (4) is 0.5 to 2 hours; Preferably, the alloy part is cooled in an inert gas after the solution treatment; Preferably, the temperature of the aging treatment in step (4) is 450-580°C; Preferably, the holding time of the aging treatment in step (4) is 0.5 to 2 hours; Preferably, the alloy part is cooled in an inert gas after the aging treatment.
8. The preparation method according to any one of claims 1 to 7, characterized in that: After step (4) is completed, the support structure on the alloy part is removed; Preferably, the support structure is removed by manual removal or mechanical removal; Preferably, after removing the support structure, polishing, sandblasting, cleaning and drying are performed in sequence to obtain the additively manufactured titanium-molybdenum alloy; Preferably, the polishing includes vibration polishing, and the roughness of the surface of the part after polishing reaches less than 6.3 μm; Preferably, the surface roughness of the part after sandblasting is less than 3.2 μm; Preferably, the cleaning is ultrasonic cleaning using an organic solvent; Preferably, the organic solvent comprises ethanol and / or acetone; Preferably, the drying comprises vacuum drying, and the drying temperature is 80 to 120° C. and the drying time is 1 to 4 hours.
9. The additively manufactured titanium-molybdenum alloy obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The titanium-molybdenum alloy includes a Ti15Mo alloy; Preferably, the composition of the titanium-molybdenum alloy includes, by mass fraction: Mo 14.5-15.5%, Fe≤0.1%, C 0.02-0.07%, O 0.07-0.10%, and the remainder is Ti and other impurity elements.
10. The use of additive manufacturing of titanium-molybdenum alloy according to claim 9, characterized in that: The additively manufactured titanium-molybdenum alloy is used as a biomedical material, preferably as a medical implant.
Citation Information
Cited By
Titanium alloy powder for selective laser melting, preparation method and application
CN120350268A
Titanium alloy powder for laser selective melting, preparation method and application
CN120350268B