Short-process 780MPa-grade thin-gauge automobile steel with high surface quality and high reaming and flanging performance and production method of short-process 780MPa-grade thin-gauge automobile steel
Through the chemical composition design and optimization of production processes with low Mn, low Nb and extremely low Si, the shortcomings of 780MPa grade automotive steel in terms of hole retraction flange performance and surface quality are solved, and high strength, high elongation and high hole retraction are achieved. The automotive steel is a high-quality automotive chassis demand and reduces production costs.
Patent Information
- Application Number
- CN202411201107.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The existing 780MPa grade high-strength automotive steel has shortcomings in terms of hole reaming and flange performance and surface quality, especially the hole reaming and flange performance of traditional duplex steel is poor, and the high Si content leads to the color difference of tiger skin and stripes, which increases the Process cost.
Using chemical composition design with low Mn content, low Nb content and extremely low Si content, combined with an optimized production process flow, including iron desulfurization, continuous casting, rolling, cooling and pickling, control chemical composition and process parameters to achieve high surface Quality and high reaming flanging performance.
Automotive steel with high surface quality and high hole reaming and flange performance has achieved tensile strength ≥780MPa, yield strength ≥660MPa, elongation ≥20%, and porosity reaming rate of pickled steel plates ≥90%, and reduced Production cost.
Smart Images

Figure BDA0005017870880000061 
Figure BDA0005017870880000062 
Figure BDA0005017870880000071
Abstract
Description
Technical Field
[0001] The invention relates to pickled high-strength automobile steel and a production method thereof, and in particular to a short-process 780MPa-grade automobile steel with high surface quality and high hole expansion and flanging performance and a production method thereof. Background Art
[0002] In the 21st century, the automotive industry has become a social need to reduce fuel consumption, CO2 and exhaust emissions. In order to adapt to this development trend, the steel industry, as a material manufacturer, has developed many types of ultra-high strength steel plates to help reduce the weight of automobiles and meet the new requirements of the automotive industry. More and more pickled automotive steel products are used to manufacture automotive parts, such as automotive suspension parts and chassis parts.
[0003] There are many automotive parts such as front / rear control arms, spring seats, etc., which are usually designed with more round holes for high-strength lightweight design and assembly requirements. These round holes need to be punched first and then expanded and flanging to obtain the final parts during the forming process. A large amount of data shows that the expansion performance and forming performance of materials are not completely equivalent. Generally speaking, the better the plasticity of steel, the better the forming performance, but it does not necessarily mean better expansion and flanging performance. For example, traditional dual-phase steel has good plasticity and good forming performance, but its expansion and flanging performance is poor, which is not suitable for the production of automotive suspension parts and chassis parts that require expansion.
[0004] CN117144254A discloses an 800MPa grade low-cost high-hole expansion performance pickled automobile steel plate and a thin slab continuous casting and rolling production method thereof, wherein the chemical composition and weight percentage content are: C 0.045%-0.065%, Si 0.40%-0.65%, Mn 1.40%-1.65%, Nb 0.020%-0.030%, Ti 0.020%-0.045%, Cr 0.40%-0.60%, P≤0.010%, S≤0.004%, and the rest are Fe and unavoidable impurities. However, 0.40% to 0.65% Si is added to the composition of the steel plate, which will form tiger stripes on the surface of the hot-rolled plate, and form stripe color differences after pickling, thereby affecting the surface quality. The requirements of automobile chassis parts for surface quality cannot be fully met. In addition, in order to reduce the risk of tiger stripe defects caused by high Si content, high-pressure water descaling is required before rolling, which will also increase the process cost. At the same time, more than 1.4% Mn and more than 0.020% Nb are added. In the current increasingly competitive market environment, the extremely low-cost composition design can better meet market demand. Summary of the invention
[0005] The present invention aims to overcome the shortcomings of the prior art and provide a thin-gauge 780MPa grade high surface quality high hole expansion and flanging performance automobile steel and a production method thereof, specifically a thickness of 1.8mm to 5.0mm, and after pickling, the tensile strength of the steel plate is ≥780MPa, the yield strength is ≥660MPa, the elongation is ≥20%, the hole expansion rate is ≥90%, and the surface quality is good, meeting the requirements of automobile chassis parts for hole expansion and flanging performance.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is:
[0007] A thin-gauge 780MPa grade steel for automobiles with high surface quality and high hole expansion and flanging performance is designed with a composition of low Mn content, low Nb content and extremely low Si content. The components and weight percentages are as follows: C 0.045-0.059%, Si 0.03-0.14%, Mn 1.05-1.38%, Nb 0.012-0.020%, Ti 0.085-0.105%, Cr 0.42-0.65%, [Cr]*[Ti]≤0.045*10 -4 (wherein [Cr] and [Ti] represent the weight percentages of Cr and Ti, respectively), N≤0.004%, S≤0.004%, and the rest are Fe and unavoidable impurities.
[0008] Preferably, the weight percentage of Si is 0.03-0.11%.
[0009] Preferably, the weight percentage of Mn is 1.08-1.36%.
[0010] Preferably, the weight percentage content of Ti is 0.088-0.103%.
[0011] Preferably, the weight percentage content of Cr is 0.43-0.56%.
[0012] Preferably, [Cr]*[Ti] is 0.035*10 -4 ~0.045*10 -4 within the range.
[0013] The present invention also provides a method for producing the above-mentioned thin-gauge 780MPa grade high surface quality and high hole expansion and flanging performance automobile steel in a short process, the steps of which are as follows:
[0014] 1) Desulfurizing, smelting and refining molten iron to obtain molten steel with target composition;
[0015] 2) After refining, continuous casting is carried out, the thickness of the casting is 57-65 mm, and the casting speed is 3.0-4.2 m / min;
[0016] 3) heating the ingot, and controlling the ingot temperature to be between 800 and 950°C, the ingot time to be between 20 and 40 minutes, and the out-of-furnace temperature to be between 1200 and 1230°C;
[0017] 4) Rolling is performed without high-pressure water descaling before rolling, and the first pass reduction rate is controlled to be 52-63%, the second pass reduction rate is 50-60%, and the final pass reduction rate is 10-16%; the rolling speed is controlled to be 8-12 m / s; medium-pressure water descaling is performed between the first and second passes, and the descaling water pressure is 200-280 bar; the final rolling temperature is controlled to be 880-920° C.;
[0018] 5) Cooling is carried out by front-stage cooling method, and the front-stage cooling rate is ≥140℃ / s;
[0019] 6) Coil the coil, and the coiling temperature is dynamically matched with the effective Ti, and the coiling temperature is controlled to be 550-1035*[effective Ti], in °C; wherein, [effective Ti]=[Ti]-3*[S]-3.42*[N], [Ti], [S], [N] are the weight percentage contents of Ti, S, and N in the steel composition, respectively;
[0020] 7) Perform pickling, and perform continuous pickling at a pickling speed of 100 to 120 m / min.
[0021] Preferably, the temperature of the ingot entering the furnace is controlled at 825-948°C, the time in the furnace is controlled at 20-33 minutes, and the temperature out of the furnace is controlled at 1205-1223°C.
[0022] The thin-gauge 780MPa grade high-surface and high-hole expansion and flanging performance automotive steel produced by the above method has a thickness of 1.8mm to 5.0mm, and the tensile strength of the steel plate after pickling is ≥780MPa, the yield strength is ≥660MPa, and the elongation is ≥20%. The hole expansion rate of the pickled steel plate is ≥90%, and the degradation rate of the pickling streak color difference defect does not exceed 0.3%; further preferably, the thickness is 1.8mm to 4.0mm, and the tensile strength of the steel plate after pickling is ≥800MPa, the yield strength is ≥680MPa, and the elongation is ≥20%. The hole expansion rate of the pickled steel plate is ≥95%, and the degradation rate of the pickling streak color difference defect does not exceed 0.25%.
[0023] The functions and mechanisms of various raw materials and main processes in the present invention are:
[0024] C: In order to ensure that the steel plate obtains a tensile strength of more than 780MPa, the carbon content of the present invention must be at least 0.045%, otherwise the tensile strength of the plate is difficult to meet the requirements. At the same time, the C content has a significant effect on the hole expansion performance. The higher the C content, the easier it is to generate cementite and pearlite. These structures are not conducive to improving the hole expansion performance. In order to increase the hole expansion rate and ensure strength, the C content range is 0.045-0.059%.
[0025] Si: Si can effectively inhibit the precipitation of cementite, which has an adverse effect on hole expansion performance. Therefore, in order to improve the hole expansion performance, the usual high hole expansion steel adds 0.30% Si to effectively inhibit the precipitation of cementite and improve the hole expansion performance. However, when the Si content exceeds 0.15%, the hot-rolled steel plate is prone to produce tiger stripes, and even after pickling, stripes will appear, affecting the surface quality of the steel plate. The important innovation of the present invention is to add a small amount or trace amount of Si element so that the steel plate can obtain good surface quality. The Si content of the present invention is controlled at 0.03-0.14%, preferably 0.03-0.11%.
[0026] Mn: Mn is the most effective element for improving strength and toughness. The Mn content of conventional 780MPa grade high-strength steel is above 1.4%, generally around 1.5%. The present invention adopts a low-cost component design, and the Mn content is controlled at 1.05-1.38%, preferably 1.08-1.36%. Compared with the Mn content of 1.5% in conventional 780MPa grade high-strength steel, the cost per ton of steel in the present invention can be reduced by 30-80 yuan.
[0027] S and N: N is an impurity element in steel. If the S and N content is too high, it will form large particles of TiS and TiN with the Ti element in the steel, thereby reducing the precipitation strengthening and fine grain strengthening effects of Ti. Therefore, the lower the content of sulfur and nitrogen elements, the better. When the strength level of the material is higher, such large particles of TiS and TiN will also have an adverse effect on the fatigue performance of the material, and must be controlled below 0.004%.
[0028] Nb: Nb is one of the important alloying elements used in the present invention. Adding Nb element can effectively refine the original austenite grain size and improve the strength and plasticity of the steel plate. At the same time, the composite precipitation of Nb and Ti can further refine the size of the precipitate and improve the strength of the material. If the Nb content exceeds 0.020%, it will lead to an increase in alloy cost, so the Nb content is controlled at 0.012-0.020%.
[0029] Ti and Cr: Ti and Cr are important alloying elements used in the present invention. Ti can play a role in fine grain strengthening and precipitation strengthening, and Cr can play a role in solid solution strengthening. Since the alloy cost of the Ti element is very low, it can replace other precious alloy elements to achieve a low-cost design. The present invention is coiled in the medium and low temperature range, and the precipitation strengthening effect of Ti cannot fully meet the required strength. At this time, a certain Cr content must be added to ensure that the tensile strength of the steel plate exceeds 780MPa. Because the contribution of Cr to strength is stable and controllable, and Ti is an active element, the performance fluctuates greatly when the Ti content is too high. Therefore, the present invention limits the Ti content according to the Cr content, that is, [Cr]*[Ti]≤0.045, so the Cr content of the present invention should be controlled at 0.42~0.65%, and the Ti content should be controlled at 0.085~0.105%. Preferably, the Cr content should be controlled at 0.43~0.56%, and the preferred Ti content should be controlled at 0.088~0.103%.
[0030] In addition to limiting the range of the above chemical components, from the perspective of improving the formability and economy of the material, the present invention does not add precious alloy elements such as Mo, V, Cu, and Ni, and achieves extreme low cost by reducing the Mn content and Nb content, adding a certain amount of relatively cheap Ti and limiting S and N, so that the added Ti can fully play the purpose of precipitation strengthening and fine grain strengthening; and because the present invention adopts a low Si composition design, high-pressure water descaling before rolling is not required. According to the above changes in composition design, the present invention also designs the continuous casting billet pulling speed, billet heating process, and coiling temperature.
[0031] The reason why the present invention controls the thickness of the ingot to be 57-65 mm and the drawing speed to be 3.0-4.2 m / min is that the present invention adopts a component design with low Mn content, low Nb content and extremely low Si content, and adds a certain amount of relatively cheap Ti. Too high a drawing speed is likely to cause ingot cracks. In order to ensure the steel flux, certain requirements are imposed on the thickness of the ingot and the drawing speed.
[0032] The reason why the present invention heats the ingot to 1200-1240°C and keeps the furnace time for 20-40 minutes is that it can ensure that the temperature of the steel plate meets the requirements of each link during the steel rolling process. In order to cooperate with the reduction of Mn and the increase of Ti, in order to ensure the precipitation and fine grain strengthening effect of Ti, the present invention specifically studies the heating temperature of the ingot. The heating temperature has a very important influence on the various properties of the finished product, and a heating temperature of more than 1200°C must be guaranteed. When the heating temperature is too low and the furnace time is too short, the Ti in the ingot cannot be completely dissolved, and in the subsequent rolling and cooling process, sufficient fine and dispersed precipitates cannot be precipitated, and the requirements of strength and hole expansion rate cannot be met; however, when the heating temperature is too high and the furnace time is too long, the original austenite grains before rolling will be coarse, which will cause the subsequent rolling process to fail to complete the complete recrystallization process of austenite, which will cause mixed crystals in the final product (i.e., the product grain size is uneven), which will seriously affect the product quality.
[0033] The reason why the present invention adopts the front-stage cooling method to immediately ultra-rapidly cool the steel plate after rolling, that is, cooling at a cooling rate of not less than 140°C / s, is to suppress the growth of grains in the steel after rolling through a high cooling rate, so that the steel can maintain a fine and uniform grain state before coiling, so that the final steel has a fine grain size and the grain size reaches level 10 or above. The coiling temperature of the present invention adopts a process of dynamically matching the effective Ti content. This is because Ti is an active element and has a great influence on mechanical properties including strength and hole expansion rate. Ti is easily combined with S and N in steel to form large particles of TiS and TiN. Such precipitates cannot make a positive contribution to strength and hole expansion rate. [Effective Ti] is generally used to evaluate the actual effect of Ti. [Effective Ti] = [Ti] - 3 * [S] - 3.42 * [N]. Effective Ti is in the range of 0.07 to 0.085%. The present invention sets the coiling temperature according to the actual value of [Effective Ti] and obtains the best mechanical properties through dynamic matching. The coiling temperature = 550-1035 * [Effective Ti]), in units of ° C.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The present invention adopts reasonable chemical composition, does not add precious alloy elements such as Mo, V, Cu, Ni, etc., but adopts a composition design with low Mn content, low Nb content and extremely low Si content to meet high surface quality requirements and low cost requirements, and ensures the performance requirements of the material by adding a certain amount of relatively low-cost Ti. On this basis, through the refined control of Ti content in the process, combined with the optimization of ingot thickness, drawing speed and heating temperature, and accurately matching the coiling temperature according to the effective Ti, the precipitation strengthening and fine grain strengthening effects of Ti are maximized, and high strength can be obtained through various strengthening effects, and high elongation and high hole expansion rate can be obtained through fine-grained ferrite and bainite structures. The requirements of high strength, high elongation and high hole expansion rate can still be met at the same time. The final thin-gauge 780MPa grade high surface quality and high hole expansion and flanging performance automotive steel has a specific thickness of 1.8mm~5.0mm, a tensile strength of ≥780MPa, a yield strength of ≥660MPa, an elongation of ≥20%, good surface quality, a pickling streak color difference defect degradation rate of no more than 0.3%, and a hole expansion rate of the pickled steel plate of ≥90%, which meets the requirements of automotive chassis parts for hole expansion and flanging performance. Compared with the traditional 780MPa grade high hole expansion steel (such as FB780, which has a higher alloy cost, a striped surface morphology, and a hole expansion rate of about 55%), the present invention adopts an extremely low-cost component design while having excellent surface quality. It can still meet the requirements of automobile chassis parts for surface quality and high hole expansion and flanging performance, and further reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the metallographic structure diagram (bainite + a small amount of ferrite) of the thin-gauge 780MPa grade high surface quality and high hole expansion and flanging performance automobile steel of the present invention. DETAILED DESCRIPTION
[0037] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.
[0038] In the present invention, the hole expansion test is carried out according to the national standard requirements. A center hole of d=10mm is punched in the center of a 150mm*150mm square plate. A conical hole expansion punch of a specified shape and size is pushed into the punched circular hole of a metal dark plate sample to carry out the hole expansion test until a crack that penetrates the thickness of the sample appears on the edge of the circular hole. The punch is stopped and the limit hole expansion rate is measured. Where λ is the limit hole expansion rate, %; D0 is the initial diameter of the punched hole (D0 = 10 mm); D H is the average diameter of the circular holes after rupture, in millimeters (mm). The hole expansion rate of the steel plate prepared by the present invention can reach more than 90%.
[0039] Example
[0040] The following describes each embodiment in detail:
[0041] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;
[0042] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;
[0043] Table 3 is a table of the performance test results of various embodiments of the present invention and comparative examples, wherein the test standards for strength and elongation are GB / T 223, and the test standard for hole expansion is GB / T 24524.
[0044] Each embodiment of the present invention produces a thin-gauge 780MPa grade steel for automobiles with high surface quality and high hole expansion and flanging performance according to the following steps. The specific steps are as follows:
[0045] 1) After desulfurization of molten iron, smelting and refining in a converter, molten steel with the target composition is obtained;
[0046] 2) Continuous casting is carried out after smelting, and the superheat of molten steel in the tundish is controlled at 15-30°C, the thickness of the billet is 57-65mm, and the billet drawing speed is 3.0-4.2m / min;
[0047] 3) heating the ingot, and controlling the ingot temperature to be between 800 and 950°C, the ingot time to be between 20 and 40 minutes, and the out-of-furnace temperature to be between 1200 and 1230°C;
[0048] 4) Rolling is performed without high-pressure water descaling before rolling, and the first pass reduction rate is controlled to be 52-63%, the second pass reduction rate is 50-60%, and the final pass reduction rate is 10-16%; the rolling speed is controlled to be 8-12 m / s; medium-pressure water descaling is performed between the first and second passes, and the descaling water pressure is 200-280 bar; the final rolling temperature is controlled to be 880-920° C.;
[0049] 5) Cooling is carried out by front-stage cooling method, and the front-stage cooling rate is ≥140℃ / s;
[0050] 6) Coil the coiling temperature, dynamically match the coiling temperature with the effective Ti, control the coiling temperature = 550-1035*[effective Ti]), the unit is ° C, substitute the effective Ti in Table 1 to obtain the corresponding coiling temperature (Note: when [effective Ti] is substituted into the formula of the coiling temperature, there is no need to substitute the unit %, for example, in Example 1, 0.0725 is substituted into the formula of the coiling temperature, and the coiling temperature = 550-1035*0.0725≈475 ° C), as shown in Table 3, in the range of 467-476 ° C;
[0051] 7) Perform pickling, and perform continuous pickling at a pickling speed of 100 to 120 m / min.
[0052] The production process of the comparative example is carried out with reference to the example, and the specific component values, process parameter values and performance tests are also shown in Tables 1, 2 and 3.
[0053] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0054]
[0055] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples
[0056]
[0057]
[0058] Table 2
[0059]
[0060] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples
[0061]
[0062] Note: The downgrade rate of pickling streak color difference defect refers to the proportion of pickled steel plates judged as downgraded products due to severe streak color difference on the surface.
[0063] It can be clearly seen from Table 3 that by adopting the chemical composition and production process of the present invention, a thin-gauge 780MPa grade high surface quality high hole expansion and flanging performance automobile steel is obtained, specifically with a thickness of 1.8mm to 5.0mm, and the tensile strength of the steel plate after pickling is ≥780MPa, the yield strength is ≥660MPa, and the elongation is ≥20%, and the hole expansion rate of the pickled steel plate is ≥90%. Compared with the traditional 780MPa grade high hole expansion steel (such as FB780, the alloy cost is high, the surface is prone to stripe-shaped color difference defects, and the hole expansion rate is about 55%), the production cost is significantly reduced, the surface quality is improved, and the degradation rate of the pickling stripe color difference defect does not exceed 0.3%. The mechanical properties can also be guaranteed, and the requirements of the automobile chassis for surface quality and high hole expansion and flanging performance are met, and the production cost is reduced. For example, in Comparative Examples 2 and Comparative Examples 3, relatively high amounts of Si are added, and the hot-rolled steel plate is easy to form tiger stripes, and the pickling stripe color difference defects are formed after pickling, which cannot meet the user's high requirements for surface quality.
[0064] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A thin gauge 780MPa grade high surface quality high hole expansion and flanging performance automotive steel, characterized in that: The components and weight percentage of the automobile steel are as follows: C 0.045-0.059%, Si 0.03-0.14%, Mn 1.05-1.38%, Nb 0.012-0.020%, Ti 0.085-0.105%, Cr 0.42-0.65%, [Cr]*[Ti]≤0.045*10 -4 , N≤0.004%, S≤0.004%, and the rest are Fe and inevitable impurities; wherein [Cr] and [Ti] represent the weight percentages of Cr and Ti respectively.
2. The thin-gauge 780MPa grade high surface quality high hole expansion and flanging performance automobile steel according to claim 1, characterized in that: The weight percentage content of Si is 0.03-0.11%.
3. The thin-gauge 780MPa grade high surface quality and high hole expansion and flanging performance automobile steel according to claim 1, characterized in that: The weight percentage of Mn is 1.08-1.36%.
4. The thin-gauge 780MPa grade high surface quality and high hole expansion and flanging performance automobile steel according to claim 1, characterized in that: The weight percentage content of Ti is 0.088-0.103%.
5. The thin-gauge 780MPa grade high surface quality and high hole expansion and flanging performance automobile steel according to claim 1, characterized in that: The weight percentage content of Cr is 0.43-0.56%.
6. A method for producing the thin-gauge 780 MPa grade high surface and high hole expansion and flanging performance automobile steel according to any one of claims 1 to 5 in a short process, the steps of which are as follows: 1) Desulfurizing, smelting and refining molten iron to obtain molten steel with target composition; 2) After refining, continuous casting is carried out, the thickness of the casting is 57-65 mm, and the casting speed is 3.0-4.2 m / min; 3) heating the ingot, and controlling the ingot temperature to be between 800 and 950°C, the ingot time to be between 20 and 40 minutes, and the out-of-furnace temperature to be between 1200 and 1230°C; 4) Rolling is performed without high-pressure water descaling before rolling, and the first pass reduction rate is controlled to be 52-63%, the second pass reduction rate is 50-60%, and the final pass reduction rate is 10-16%; the rolling speed is controlled to be 8-12 m / s; medium-pressure water descaling is performed between the first and second passes, and the descaling water pressure is 200-280 bar; the final rolling temperature is controlled to be 880-920° C.; 5) Cooling is carried out by front-stage cooling method, and the front-stage cooling rate is ≥140℃ / s; 6) Coil the coil, and the coiling temperature is dynamically matched with the effective Ti, and the coiling temperature is controlled to be 550-1035*[effective Ti], in °C; wherein, [Effective Ti] = [Ti]-3*[S]-3.42*[N], where [Ti], [S], and [N] are the weight percentages of Ti, S, and N in the steel composition, respectively; 7) Perform pickling, and perform continuous pickling at a pickling speed of 100 to 120 m / min.
7. The method for producing thin-gauge 780MPa grade high surface and high hole expansion and flanging performance automobile steel in a short process according to claim 6, characterized in that: The ingot entering furnace temperature is controlled at 825-948°C, the ingot staying time is controlled at 20-33min, and the ingot exiting furnace temperature is controlled at 1205-1223°C.
8. The thin gauge 780MPa grade high surface and high hole expansion and flanging performance automobile steel produced according to claim 6 or 7, characterized in that: The thickness is 1.8mm~5.0mm, the tensile strength is ≥780MPa, the yield strength is ≥660MPa, the elongation is ≥20%, the hole expansion rate is ≥90%, and the degradation rate of pickling stripe color difference defects does not exceed 0.3%.
9. The thin gauge 780MPa grade high surface and high hole expansion and flanging performance automobile steel produced according to claim 6 or 7, characterized in that: The thickness is 1.8mm~4.0mm, the tensile strength is ≥800MPa, the yield strength is ≥680MPa, the elongation is ≥20%, the hole expansion rate is ≥95%, and the degradation rate of pickling stripe color difference defects does not exceed 0.25%.
Citation Information
Patent Citations
780 MPa-grade hot-rolled dual-phase steel with excellent hole expanding performance and preparation method of 780 MPa-grade hot-rolled dual-phase steel
CN113005367A
800MPa-grade low-cost high-broaching-performance acid-pickled automobile steel plate and thin slab continuous casting and rolling production method thereof
CN117144254A
Production method of high tensile hot rolled steel plate for working
JP2001089811A