Preparation method of ultraviolet-proof, shielding, flame-retardant, low-temperature-resistant, acid-resistant and alkali-resistant filament and fabric

By melting the metal powder and polytetrafluoroethylene into one, low-temperature and ultraviolet-resistant conductive fabric is prepared, which solves the performance problems of the spacesuit in high-temperature, low-temperature, acid and alkali environments, and maintains the shielding effect after bending and folding , ensure the safety of astronauts.

CN119061508APending Publication Date: 2024-12-03BOYUE NEW MATERIAL TECHNOLOGY (JIANGSU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411206815.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing spacesuit materials cannot maintain performance in high temperature, low temperature, acid, alkali, ultraviolet rays and electromagnetic radiation environments, and metal powders are prone to fall off during processing and storage, resulting in a decrease in shielding efficiency.

Method used

Ultrafine polytetrafluoroethylene filaments are melted into one with metal powders (such as silver, nickel, copper, graphene), and flame retardant, low temperature resistant and anti-corrosion through constant temperature maturation, hot extrusion, stretching and winding processes. Ultraviolet conductive fabric ensures that the shielding performance does not decrease after being bent and folded.

Benefits of technology

The corrosion resistance and conductive shielding performance in high-temperature, low-temperature, acid, alkali, ultraviolet and electromagnetic radiation environments are achieved, ensuring the safety and service life of the space suit, and avoiding the problem of metal powder falling off.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061508A_ABST
    Figure CN119061508A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of material processing, in particular to a preparation method of an anti-ultraviolet shielding flame-retardant low-temperature-resistant acid-alkali-resistant filament and fabric, which comprises the following steps: firstly, putting a polytetrafluoroethylene raw material into a vibration screen for screening, putting polytetrafluoroethylene fine powder into a universal stirrer after the screening is completed, and uniformly stirring; and aviation kerosene is added into the universal stirrer. Silver powder, nickel powder, copper powder, graphene powder and the like, polytetrafluoroethylene emulsion and ultra-thin filaments are fused into a whole, metal powder is not firmly embedded in a polytetrafluoroethylene material, and therefore the metal powder does not fall off after being bent and folded, and it is guaranteed that the shielding effectiveness is not reduced; through polymerization with metal silver, nickel, copper, graphene and the like, the conductive shielding filament also has the functions of flame retardance, low temperature resistance, corrosion resistance and ultraviolet resistance, the body safety of astronauts can be effectively guaranteed, and the conductive shielding filament can be washed with water and reused.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material processing, and in particular to a method for preparing ultraviolet-proof, shielding, flame-retardant, low-temperature-resistant, acid- and alkali-resistant filament and fabric. Background Art

[0002] Space suits need to adapt to high temperatures (above +200 degrees) and low temperatures (below -150 degrees), acid, alkali, salt corrosion, UV and electromagnetic radiation, and be ultra-thin and ultra-light. Textile colleges and universities use a variety of high-performance fibers such as PE, aramid, polyimide, carbon fiber, basalt, etc., but the above high-performance fibers have some shortcomings and cannot meet the technical requirements. For example, PE has ultra-high strength and is resistant to low temperatures but not high temperatures, and will deform and melt at 100 degrees; aramid is resistant to alkali but not acid, and even less resistant to UV radiation; polyimide is resistant to acid but not alkali; carbon fiber and basalt are brittle and easy to break, cannot be woven, are allergic to the human body, cannot be made into clothing, and metal powder cannot be dissolved into the fiber structure.

[0003] At present, there are metal stainless steel fiber fabrics and equipment and fabrics coated with metal silver, nickel, copper powder and other materials. The shielding efficiency of metal stainless steel fabrics in the band above 3GHZ cannot meet the electromagnetic radiation function of the sky, and it cannot be used for a long time because the diameter of stainless steel fiber is smaller than the pores of human skin, causing allergic reactions. The powder fabrics coated with silver, nickel, copper, graphene, etc. need to be bent, folded or washed during processing and storage, which causes the metal powder to fall off, and the shielding efficiency decreases, and cannot meet the original quality requirements. In order to solve the bottleneck problem of the decline in shielding efficiency caused by the fall of metal powder, the present invention proposes a method for preparing a UV-proof shielding flame-retardant low-temperature-resistant acid-base-resistant filament and fabric, using ultra-fine denier polytetrafluoroethylene filaments and emulsion as raw materials to prepare permanent flame-retardant, low-temperature-resistant, UV-proof, acid-resistant and alkali-resistant electromagnetic shielding mixed and fused metal silver, nickel, copper, graphene and other ultra-fine denier space suit filaments. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing an anti-ultraviolet shielding flame-retardant low-temperature resistant acid-base resistant filament and fabric, which has the functions of flame retardancy, low-temperature resistance, corrosion resistance and ultraviolet resistance, and can be bent and folded arbitrarily while the conductive shielding and anti-ultraviolet performance does not decrease. It solves the problem that the current metal stainless steel fiber fabric needs to be bent, folded or washed during processing and storage and wearing, which easily causes metal powder to fall off and reduces the shielding performance.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a UV-proof, flame-retardant, low-temperature-resistant, acid- and alkali-resistant filament and fabric, the method comprising the following steps:

[0006] S1: First, the polytetrafluoroethylene raw material is placed in a vibrating screen for screening. After the screening is completed, the polytetrafluoroethylene fine powder is placed in a universal mixer, and aviation kerosene is added to the universal mixer. Under the operation of the universal mixer, the polytetrafluoroethylene fine powder and the aviation kerosene are dissolved together to obtain a polytetrafluoroethylene mixture;

[0007] S2: The polytetrafluoroethylene mixture is subjected to a constant temperature aging treatment, and after completion, it is put into a hot extruder for heating and extrusion into a semi-finished round rod, and the semi-finished round rod is subjected to a degreasing and calendering treatment to obtain a semi-finished film blank;

[0008] S3: taking polytetrafluoroethylene emulsion and adding metal powder and graphene powder thereto, stirring evenly to obtain a mixed solution, placing the mixed solution in a heating solution box for heating and standby use, and after the semi-finished film blank is heated and cut into semi-finished polytetrafluoroethylene filaments, passing through the rear roller and the heating solution box in sequence;

[0009] S4: The polytetrafluoroethylene filament is stretched once and passed through the bell mouth. The polytetrafluoroethylene filament is heated and melted in the second stretching oven and passed through the bell mouth. Under the action of the bell mouth, the filament is pulled out and wound through the front roller according to the designed diameter. The front roller and the rear roller stretch the filament faster and slower to obtain the finished polytetrafluoroethylene filament;

[0010] S5: Circulating water cools and shrinks the PTFE filament, after it is cooled and shaped, it is wound and inspected before leaving the factory.

[0011] Preferably, in step S1, the mesh size of the vibration screen is selected to be 20 meshes to screen out the polytetrafluoroethylene fine powder.

[0012] Preferably, in step S1, the rotation speed of the universal mixer is 60-100 r / min.

[0013] Preferably, in step S2, the parameters of the constant temperature aging include: the aging temperature is controlled at 360-375° C., and the aging time is 8-12 hours.

[0014] Preferably, in step S2, the temperature of the hot extruder is controlled at 380-400°C, and the temperature is maintained constant for continuous extrusion.

[0015] Preferably, in step S2, the semi-finished round rod is degreased and placed in a degreasing oven, the degreasing temperature is controlled at 250-300°C, and the semi-finished round rod is calendered using rollers during calendering to obtain a semi-finished film blank of desired width and thickness.

[0016] Preferably, in step S3, the solid content of the polytetrafluoroethylene emulsion is 60%, and the metal powder includes but is not limited to silver, nickel, and copper powder.

[0017] Preferably, in step S4, a speed regulating switch or a frequency converter is installed at each of the front roller and the rear roller, and the drafting is changed from coarse to fine by speeding up the front roller and slowing down the rear roller under the condition of controlling the speed ratio, so that the 100D filament is drafted into a 40D filament.

[0018] Preferably, in step S4, the filaments and the solution containing silver, nickel, copper and graphene powders heated to high temperature are dissolved together, and the filaments finally obtained are 55D±10D.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The method for preparing the anti-ultraviolet shielding flame-retardant, low-temperature-resistant, acid-base-resistant filaments and fabrics proposed by the present invention is to melt silver, nickel, copper, graphene and other powders and polytetrafluoroethylene emulsion and ultrafine filaments into one, so that the metal powder is not firmly embedded in the polytetrafluoroethylene material, so that it does not fall off after bending and folding to ensure that the shielding efficiency is not reduced. Since polytetrafluoroethylene has flame retardant and corrosion-resistant functions, it is polymerized with metal silver, nickel, copper, graphene and the like, so that the conductive shielding filaments also have flame retardant, low-temperature-resistant, corrosion-resistant and ultraviolet-resistant functions, solves the problem of low ultrafine pole strength of mixed spinneret filaments, and the current metal stainless steel fiber fabrics need to be bent, folded or washed during processing and storage and wearing, which easily causes metal powder to fall off and the shielding efficiency to decrease. The breaking strength of the original polytetrafluoroethylene filaments is retained, and because they are melted into one, they can be bent and folded arbitrarily, and the conductive shielding anti-ultraviolet efficiency is not reduced, which can effectively protect the body safety of astronauts. The conductive shielding filaments can be washed and reused, and have the advantages of environmentally friendly use and long service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a flow chart of the preparation method. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] A method for preparing ultraviolet-proof, shielding, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric, the method comprising the following steps:

[0025] S1: First, the polytetrafluoroethylene raw material is loaded into a vibrating screen for screening. After the screening is completed, the polytetrafluoroethylene fine powder is put into a universal mixer, and aviation kerosene is added to the universal mixer. Under the operation of the universal mixer, the polytetrafluoroethylene fine powder and the aviation kerosene are dissolved together to obtain a polytetrafluoroethylene mixture.

[0026] In this embodiment, the mesh size of the vibration screen is selected to be 20 meshes to screen out the polytetrafluoroethylene fine powder, wherein the rotation speed of the universal mixer is 80r / min to ensure the uniformity of stirring.

[0027] S2: The polytetrafluoroethylene mixture is subjected to a constant temperature aging treatment, and after completion, it is put into a hot extruder for heating and extrusion into a semi-finished round rod, and the semi-finished round rod is subjected to a degreasing and calendering treatment to obtain a semi-finished film blank.

[0028] In this embodiment, during the constant temperature aging treatment, the aging temperature is controlled at 360°C and the aging time is 12 hours to avoid the melting of polytetrafluoroethylene due to excessive temperature. The temperature of the hot extruder is controlled at 380°C and the temperature is kept constant for continuous extrusion. According to the product form and requirements of the polytetrafluoroethylene round rod, appropriate temperature and pressure are set and maintained for a certain period of time to allow the raw materials to fully melt and flow to form the desired product form. The semi-finished round rod is degreased and placed in a degreasing oven. The degreasing temperature is controlled at 300°C. During the calendering treatment, the semi-finished round rod is calendered with a roller to obtain a semi-finished film blank of the desired width and thickness.

[0029] S3: Take polytetrafluoroethylene emulsion and add metal powder and graphene powder thereto, stir evenly to obtain a mixed solution, place the mixed solution in a heating solution box for heating and standby use, and after the semi-finished film blank is heated and cut into semi-finished polytetrafluoroethylene filaments, pass through the rear roller and the heating solution box in sequence.

[0030] In this embodiment, the solid content of the polytetrafluoroethylene emulsion is 60%, and the metal powder includes but is not limited to silver, nickel, and copper powder.

[0031] S4: The polytetrafluoroethylene filament is stretched once and passed through the bell mouth. The polytetrafluoroethylene filament is heated and melted in the second stretching oven and then pulled out and wound through the front roller according to the designed diameter under the action of the bell mouth. The front roller and the rear roller stretch the filament faster and slower to obtain the finished polytetrafluoroethylene filament.

[0032] In this embodiment, a speed regulating switch or a frequency conversion device is installed at the front roller and the rear roller respectively, and the drafting is changed from coarse to fine by speeding up the front roller and slowing down the rear roller under the condition of controlling the speed ratio, so that the 100D filament is stretched into a 40D filament, and the filament and the solution containing silver, nickel, copper and graphene powder are dissolved into one after being heated to high temperature, and the final filament is 55D±10D.

[0033] S5: Circulating water cools and shrinks the PTFE filament, after it is cooled and shaped, it is wound and inspected before leaving the factory.

[0034] Embodiment 2:

[0035] A method for preparing ultraviolet-proof, shielding, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric, the method comprising the following steps:

[0036] S1: First, the polytetrafluoroethylene raw material is loaded into a vibrating screen for screening. After the screening is completed, the polytetrafluoroethylene fine powder is put into a universal mixer, and aviation kerosene is added to the universal mixer. Under the operation of the universal mixer, the polytetrafluoroethylene fine powder and the aviation kerosene are dissolved together to obtain a polytetrafluoroethylene mixture.

[0037] In this embodiment, the mesh size of the vibration screen is selected to be 20 meshes to screen out the polytetrafluoroethylene fine powder, wherein the rotation speed of the universal mixer is 100 r / min to ensure the uniformity of stirring.

[0038] S2: The polytetrafluoroethylene mixture is subjected to a constant temperature aging treatment, and after completion, it is put into a hot extruder for heating and extrusion into a semi-finished round rod, and the semi-finished round rod is subjected to a degreasing and calendering treatment to obtain a semi-finished film blank.

[0039] In this embodiment, during the constant temperature aging treatment, the aging temperature is controlled at 375°C and the aging time is 8 hours to avoid the melting of polytetrafluoroethylene due to excessive temperature. The temperature of the hot extruder is controlled at 400°C and the temperature is kept constant for continuous extrusion. According to the product form and requirements of the polytetrafluoroethylene round rod, appropriate temperature and pressure are set and maintained for a certain period of time to allow the raw materials to fully melt and flow to form the desired product form. The semi-finished round rod is degreased and placed in a degreasing oven. The degreasing temperature is controlled at 260°C. During the calendering treatment, the semi-finished round rod is calendered with a roller to obtain a semi-finished film blank of the desired width and thickness.

[0040] S3: Take polytetrafluoroethylene emulsion and add metal powder and graphene powder thereto, stir evenly to obtain a mixed solution, place the mixed solution in a heating solution box for heating and standby use, and after the semi-finished film blank is heated and cut into semi-finished polytetrafluoroethylene filaments, pass through the rear roller and the heating solution box in sequence.

[0041] In this embodiment, the solid content of the polytetrafluoroethylene emulsion is 60%, and the metal powder includes but is not limited to silver, nickel, and copper powder.

[0042] S4: The polytetrafluoroethylene filament is stretched once and passed through the bell mouth. The polytetrafluoroethylene filament is heated and melted in the second stretching oven and then pulled out and wound through the front roller according to the designed diameter under the action of the bell mouth. The front roller and the rear roller stretch the filament faster and slower to obtain the finished polytetrafluoroethylene filament.

[0043] In this embodiment, a speed regulating switch or a frequency conversion device is installed at the front roller and the rear roller respectively, and the drafting is changed from coarse to fine by speeding up the front roller and slowing down the rear roller under the condition of controlling the speed ratio, so that the 100D filament is stretched into a 40D filament, and the filament and the solution containing silver, nickel, copper and graphene powder are dissolved into one after being heated to high temperature, and the final filament is 55D±10D.

[0044] S5: Circulating water cools and shrinks the PTFE filament, after it is cooled and shaped, it is wound and inspected before leaving the factory.

[0045] In summary, the present invention melts silver, nickel, copper, graphene and other powders and polytetrafluoroethylene emulsion plus ultrafine filaments into one, so that the metal powder is not firmly embedded in the polytetrafluoroethylene material, so that it does not fall off after bending and folding to ensure that the shielding effectiveness is not reduced. Since polytetrafluoroethylene has flame retardant and corrosion resistant functions, it is polymerized with metal silver, nickel, copper, graphene and the like, so that the conductive shielding filaments also have flame retardant, low temperature resistance, corrosion resistance, and UV resistance. The problem of low ultrafine pole strength of mixed spinneret filaments and the problem that the current metal stainless steel fiber fabrics need to be bent, folded or washed during processing and storage and wearing, which easily causes the metal powder to fall off and the shielding effectiveness to decrease. The breaking strength of the original polytetrafluoroethylene filaments is retained, and because it is melted into one, it can be bent and folded arbitrarily while the conductive shielding anti-ultraviolet performance is not reduced, which can effectively protect the safety of astronauts. The conductive shielding filaments can be washed and reused, and have the advantages of environmentally friendly use and long service life.

[0046] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0047] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing UV-proof, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric, characterized in that: The method comprises the following steps: S1: First, the polytetrafluoroethylene raw material is placed in a vibrating screen for screening. After the screening is completed, the polytetrafluoroethylene fine powder is placed in a universal mixer, and aviation kerosene is added to the universal mixer. Under the operation of the universal mixer, the polytetrafluoroethylene fine powder and the aviation kerosene are dissolved together to obtain a polytetrafluoroethylene mixture; S2: The polytetrafluoroethylene mixture is subjected to a constant temperature aging treatment, and after completion, it is put into a hot extruder for heating and extrusion into a semi-finished round rod, and the semi-finished round rod is subjected to a degreasing and calendering treatment to obtain a semi-finished film blank; S3: taking polytetrafluoroethylene emulsion and adding metal powder and graphene powder thereto, stirring evenly to obtain a mixed solution, placing the mixed solution in a heating solution box for heating and standby use, and after the semi-finished film blank is heated and cut into semi-finished polytetrafluoroethylene filaments, passing through the rear roller and the heating solution box in sequence; S4: The polytetrafluoroethylene filament is stretched once and passed through the bell mouth. The polytetrafluoroethylene filament is heated and melted in the second stretching oven and passed through the bell mouth. Under the action of the bell mouth, the filament is pulled out and wound through the front roller according to the designed diameter. The front roller and the rear roller stretch the filament faster and slower to obtain the finished polytetrafluoroethylene filament; S5: Circulating water cools and shrinks the PTFE filament, after it is cooled and shaped, it is wound and inspected before leaving the factory.

2. The method for preparing a UV-proof, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric according to claim 1, characterized in that: In the step S1, the mesh size of the vibration screen is selected to be 20 meshes to screen out the polytetrafluoroethylene fine powder.

3. The method for preparing a UV-proof, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric according to claim 1, characterized in that: In the step S1, the rotation speed of the universal mixer is 60-100 r / min.

4. The method for preparing a UV-proof, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric according to claim 1, characterized in that: In step S2, the parameters of the constant temperature aging include: the aging temperature is controlled at 360-375° C., and the aging time is 8-12 hours.

5. The method for preparing the UV-proof, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric according to claim 1, characterized in that: In step S2, the temperature of the hot extruder is controlled at 380-400°C, and the extrusion is continued while maintaining the temperature constant.

6. The method for preparing the anti-ultraviolet shielding flame-retardant low-temperature resistant acid-base resistant filament and fabric according to claim 1, characterized in that: In the step S2, the semi-finished round rod is degreased and placed in a degreasing oven, the degreasing temperature is controlled at 250-300°C, and the semi-finished round rod is calendered using a roller during calendering to obtain a semi-finished film blank of desired width and thickness.

7. The method for preparing the anti-ultraviolet shielding flame retardant low temperature resistant acid and alkali resistant filament and fabric according to claim 1, characterized in that: In the step S3, the solid content of the polytetrafluoroethylene emulsion is 60%, and the metal powder includes but is not limited to silver, nickel, and copper powder.

8. The method for preparing the UV-proof, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric according to claim 1, characterized in that: In step S4, a speed regulating switch or a frequency converter is installed at each of the front roller and the rear roller, and the drafting is changed from coarse to fine by speeding up the front roller and slowing down the rear roller under the condition of controlling the speed ratio, so that the 100D filament is drafted into a 40D filament.

9. The method for preparing the UV-proof, flame-retardant, low-temperature-resistant, acid-base-resistant filament and fabric according to claim 1, characterized in that: In the step S4, the filament and the solution containing silver, nickel, copper and graphene powder after being heated to high temperature are dissolved together, and the filament finally obtained is 55D±10D.