Food paperboard and preparation method thereof
By using the laminated structure design of modified polyacrylate water-based coatings with core-shell structure in food jam paper, the problem of high heat sealing temperature and adhesion in food packaging paper is solved, and suitable heat sealing is achieved Temperature and stable adhesion properties are suitable for food packaging.
Patent Information
- Application Number
- CN202410975822.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-19
AI Technical Summary
In food packaging paper, water-based polyacrylate emulsions have problems such as leakage due to excessive heat sealing temperature, easy to stick after water absorption, and self-adhesion and damage coating integrity due to high temperatures. It is difficult to achieve low heat sealing temperature and not Reverse sticking requirements.
The laminated structure design of modified polyacrylate water-based coating A and modified polyacrylate water-based coating B with core-shell structure is 8-10g/m2 and 0.5-2g/m2 respectively, forming a heat seal The functional layer and the anti-adhesive layer are dried by five-section hot air tanks to control the heat sealing temperature and adhesion properties of the cardboard.
The suitable heat sealing temperature of food jam paper is achieved, while improving the adhesion performance of the paper, avoiding leakage and self-adhesion, and ensuring the stability and barrier performance of the paper cup in high temperature and high humidity environments.
Smart Images

Figure CN119061732A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of food cardboard preparation technology, and specifically to a food cardboard and a preparation method thereof. Background Art
[0002] At present, due to the influence of the national plastic ban policy on polyethylene, polypropylene and other coated disposable packaging papers, water-based coatings have become an important substitute for coated paper. In recent years, taking water-based coating materials as an example, compared with the traditional PE coating 18g / m2 process, while meeting the barrier performance requirements, water-based coatings only require a coating amount of (5-10) g / m2. The lower coating thickness, on the one hand, reduces the application amount of barrier coatings, and on the other hand, the coating is easier to break and degrade. Food packaging paper with water-based coatings has the advantages of saving resources, being repulpable and recyclable.
[0003] After being coated into a film, polyacrylate emulsion has good permeability, high elasticity, biodegradability, acid resistance, chemical resistance and aging resistance. However, polyacrylate emulsion itself has the disadvantages of poor water resistance, poor adhesion, brittleness at low temperature and viscosity at high temperature, which limits the application of polyacrylate emulsion. At present, the modification of water-based polyacrylate emulsion has greatly improved the application range of emulsion coatings.
[0004] Among food packaging cardboards, paper cups have higher performance requirements and food safety requirements for water-based polyacrylate emulsions due to their high barrier and processing performance requirements. Paperboards coated with water-based polyacrylate emulsions usually have the following application difficulties: 1. The heat sealing temperature of the cup bottom is too high, resulting in the heat sealing of the paper cup bottom not being strong, and leakage occurs when the paper cup is filled with liquid. The heat sealing temperature exceeds the set temperature of the cup making machine, and too high a temperature (above 400 degrees) will carbonize and yellow the paper substrate; 2. It is easy to become sticky after absorbing water and getting wet, so that the paper cup sheets are sticky and form blocks; 3. The high-temperature stickiness makes the cup tube easy to self-adhere under high temperature and high humidity conditions after the cup is formed, resulting in poor cup pulling and damage to the integrity of the coating. It is difficult for a single polyacrylate emulsion to achieve the requirements of low heat sealing temperature and no re-sticking. By adding a certain amount of inorganic fillers such as talcum powder with high slipperiness to the polyacrylate emulsion, the adhesion of polyacrylate can be improved to a certain extent, but the inorganic fillers on the coating surface will still affect the heat sealing temperature and bonding strength of the cup sheets when the cup is formed. Summary of the invention
[0005] A first aspect of an embodiment of the present application provides a method for preparing food card paper, the method comprising:
[0006] Provide base paper;
[0007] Applying a modified polyacrylate water-based coating A on the base paper to form a heat-sealing functional layer; wherein the modified polyacrylate water-based coating A is a polymer emulsion with a core-shell structure;
[0008] A modified polyacrylate water-based coating B is coated on the heat-sealing functional layer to form an anti-blocking layer.
[0009] In some embodiments, the core of the modified polyacrylate water-based coating A is a polymer of ethylene-butyl acrylate, and the polymerized monomers of the shell structure are ethylene, butyl acrylate and methyl acrylate.
[0010] In some embodiments, in the ethylene-butyl acrylate polymer, the ratio of ethylene to butyl acrylate is 4-6:6-4; in the polymer monomer of the shell structure, the ratio of ethylene, butyl acrylate and methyl acrylate is 3:5:2.
[0011] In some embodiments, the modified polyacrylate water-based coating B includes methyl methacrylate and butyl acrylate polymerized.
[0012] In some embodiments, the ratio of the methyl methacrylate to the butyl acrylate is 7:3.
[0013] In some embodiments, the modified polyacrylate water-based coating B further includes octadecyl acrylate, and the added amount of octadecyl acrylate is 5-8% of the total amount of the methyl methacrylate and the butyl acrylate.
[0014] In some embodiments, the coating amount of the modified polyacrylate water-based coating A is 8-10 g / m2, and the coating amount of the modified polyacrylate water-based coating B is 0.5-2 g / m2.
[0015] In some embodiments, the thickness of the heat-sealing functional layer is 8-10 um; the thickness of the anti-adhesion layer is 0.5-2 um.
[0016] In some embodiments, the preparation method further includes a drying process, wherein the drying process uses a five-stage hot air oven drying, and the drying temperatures are 110 / 120 / 130 / 110 / 100°C, respectively.
[0017] In a second aspect, an embodiment of the present application provides a food paperboard, which is prepared by the preparation method described in the above embodiment.
[0018] The method for preparing food cardboard provided in the embodiment of the present application develops two modified water-based polyacrylate emulsions. Through the design of the coating structure, a modified polyacrylate film is formed on the surface of the cardboard by a coating composite method to prepare food card packaging paper, so that the food cardboard has a more suitable cup heat sealing temperature while improving paper adhesion. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 It is a schematic flow chart of an embodiment of a method for preparing food card paper of the present application;
[0021] Figure 2 It is a schematic diagram of the structure after a heat-sealing functional layer is formed on the base paper;
[0022] Figure 3 This is a schematic diagram of the stacked structure of an embodiment of the food card paper of the present application;
[0023] Figure 4 It is a flow chart of another embodiment of the method for preparing food card paper of the present application. DETAILED DESCRIPTION
[0024] The present application is further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present application, but are not intended to limit the scope of the present application. Similarly, the following examples are only some embodiments of the present application rather than all embodiments, and all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0025] The terms "first", "second", and "third" in the embodiments of the present application are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second", and "third" can expressly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the embodiments of the present application, all directional indications (such as up, down, left, right, front, back...) are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. The terms "including" and "having" in the embodiments of the present application and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product, or device that includes a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or components inherent to these processes, methods, products, or devices.
[0026] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0027] The present application provides a method for preparing food card paper. Figure 1 , Figure 1 It is a flow chart of an embodiment of a method for preparing food card paper of the present application, and the preparation method includes but is not limited to the following steps.
[0028] Step S100, providing base paper.
[0029] The base paper used in this embodiment is acid-sizing uncoated food card base paper.
[0030] Step S200, coating the modified polyacrylate water-based coating A on the base paper to form a heat-sealing functional layer.
[0031] See also Figure 2 , Figure 2 It is a schematic diagram of the structure after a heat-sealing functional layer is formed on base paper, in which 110 is base paper and 120 is the heat-sealing functional layer.
[0032] Optionally, the modified polyacrylate water-based coating A in this embodiment is a polymer emulsion with a core-shell structure. Wherein, the core of the modified polyacrylate water-based coating A is a polymer of ethylene-butyl acrylate, and in the polymer of ethylene-butyl acrylate, the ratio of ethylene to butyl acrylate is 4-6:6-4. The polymerized monomers of the shell structure are ethylene, butyl acrylate and methyl acrylate, wherein the ratio of ethylene, butyl acrylate and methyl acrylate is 3:5:2. Soft monomers and hard monomers are selected for polymerization to obtain a suitable glass transition temperature, and the solid content of the modified polyacrylate water-based coating A emulsion is 38-40%. Wherein, the coating amount of the modified polyacrylate water-based coating A is 8-10g / m2.
[0033] Please continue reading Figure 1 The preparation method in this embodiment further includes: step S300, coating a modified polyacrylate water-based coating B on the heat-sealing functional layer to form an anti-adhesive layer.
[0034] See also Figure 3 , Figure 3 1 is a schematic diagram of the stacked structure of an embodiment of the food card paper of the present application, wherein the anti-adhesion layer 130 is disposed on the sealing function layer 120 .
[0035] Wherein, the modified polyacrylate water-based coating B in this embodiment includes methyl methacrylate and butyl acrylate, and the ratio of methyl methacrylate to the butyl acrylate is 7:3. Optionally, the modified polyacrylate water-based coating B can also include octadecyl acrylate, and the addition amount of octadecyl acrylate is 5-8% of the total of methyl methacrylate and butyl acrylate. The solid content of the modified polyacrylate water-based coating B emulsion is controlled at about 20%. Wherein, the coating amount of the modified polyacrylate water-based coating B is 0.5-2g / m2. Both coatings (modified polyacrylate water-based coating A and modified polyacrylate water-based coating B) can be applied by scraper.
[0036] The design of the two coatings and coating thicknesses is that the coating thickness of modified polyacrylate A is controlled at 8-10um, which has good water and oil barrier properties. The low Tg characteristics of the coating enable the coating to melt quickly and have fluidity during the heat sealing process of the paperboard. During the knurling process of the bottom of the paper cup, the molten coating can quickly penetrate into the fiber pores on the back of the paperboard. After the knurling is completed, the coating temperature drops in the absence of heating, and the coating can be quickly solidified to play a bonding and barrier role. The coating thickness of modified polyacrylate water-based coating B is controlled at 0.5-2um. It has a long-chain hydrophobic monomer, so it has good water resistance after film formation, and is not prone to self-adhesion in high temperature and high humidity environments. The melting temperature is slightly higher, but the coating thickness is thinner. After the coating A melts, the coating will also be destroyed. It will enter the fiber pores under the heat sealing extrusion of the paper cup machine film, and has little effect on the heat sealing temperature.
[0037] The structural characteristics of the modified polyacrylate water-based coating A enable the shell structure to still cover part of the emulsion seeds after the coating process of demulsification and film formation, which can inhibit the self-adhesion of the emulsion seeds under high temperature and high humidity conditions, and make the coating have good compatibility with the modified polyacrylate water-based coating B, so that the two coatings can have good bonding strength, and there will be no separation and peeling problems when the cup is filled with hot water. During the heat sealing process of the cardboard, the seed structure is softer, making the entire coating easy to melt and have good fluidity, thus having good heat sealing performance. The regular linear structure of the ethylene polymerization block in the monomer makes the polymers in the film closer together, and has good water and oil resistance.
[0038] Modified polyacrylate water-based coating B is modified by adding octadecyl acrylate. The hydrophobic alkyl side chains can make the coating surface have good hydrophobicity. Under high temperature and high humidity, the alkyl side chains will not absorb water vapor and cause adhesion between the two cardboards. It contains the same polymerization monomer as the water-based coating B, so that the two coatings have good compatibility.
[0039] The method for preparing food cardboard provided in the embodiment of the present application develops two modified water-based polyacrylate emulsions. Through the design of the coating structure, a modified polyacrylate film is formed on the surface of the cardboard by a coating composite method to prepare food card packaging paper, so that the food cardboard has a more suitable cup heat sealing temperature while improving paper adhesion.
[0040] See also Figure 4 , Figure 4 It is a flow chart of another embodiment of the method for preparing food card paper of the present application, and the preparation method includes but is not limited to the following steps.
[0041] Step S100, providing base paper.
[0042] The base paper in this embodiment can also be an uncoated food card base paper with acid sizing.
[0043] Step S200, coating the modified polyacrylate water-based coating A on the base paper to form a heat-sealing functional layer.
[0044] Optionally, the modified polyacrylate water-based coating A in this embodiment can also be a polymer emulsion with a core-shell structure. Among them, the core of the modified polyacrylate water-based coating A is a polymer of ethylene-butyl acrylate, and in the polymer of ethylene-butyl acrylate, the ratio of ethylene to butyl acrylate is 4-6:6-4. The polymerized monomers of the shell structure are ethylene, butyl acrylate and methyl acrylate, and the ratio of ethylene, butyl acrylate and methyl acrylate is 3:5:2. Soft monomers and hard monomers are selected for polymerization to obtain a suitable glass transition temperature, and the solid content of the modified polyacrylate water-based coating A emulsion is 38-40%. Among them, the coating amount of the modified polyacrylate water-based coating A is 8-10g / m2.
[0045] Please continue reading Figure 4 The preparation method in this embodiment further includes: step S300, coating a modified polyacrylate water-based coating B on the heat-sealing functional layer to form an anti-adhesive layer.
[0046] Among them, the modified polyacrylate water-based coating B in this embodiment can also be formed by the polymerization of methyl methacrylate and butyl acrylate, and the ratio of methyl methacrylate to the butyl acrylate is 7:3. Optionally, the modified polyacrylate water-based coating B can also include octadecyl acrylate, and the addition amount of octadecyl acrylate is 5-8% of the total of methyl methacrylate and butyl acrylate. The solid content of the modified polyacrylate water-based coating B emulsion is controlled at about 20%. Among them, the coating amount of the modified polyacrylate water-based coating B is 0.5-2g / m2. Both coatings (modified polyacrylate water-based coating A and modified polyacrylate water-based coating B) can be applied by scraper.
[0047] The design of the two coatings and coating thicknesses is that the coating thickness of modified polyacrylate A is controlled at 8-10um, which has good water and oil barrier properties. The low Tg characteristics of the coating enable the coating to melt quickly and have fluidity during the heat sealing process of the paperboard. During the knurling process of the bottom of the paper cup, the molten coating can quickly penetrate into the fiber pores on the back of the paperboard. After the knurling is completed, the coating temperature drops in the absence of heating, and the coating can be quickly solidified to play a bonding and barrier role. The coating thickness of modified polyacrylate water-based coating B is controlled at 0.5-2um. It has a long-chain hydrophobic monomer, so it has good water resistance after film formation, and is not prone to self-adhesion in high temperature and high humidity environments. The melting temperature is slightly higher, but the coating thickness is thinner. After the coating A melts, the coating will also be destroyed. It will enter the fiber pores under the heat sealing extrusion of the paper cup machine film, and has little effect on the heat sealing temperature.
[0048] The structural characteristics of the modified polyacrylate water-based coating A enable the shell structure to still cover part of the emulsion seeds after the coating process of demulsification and film formation, which can inhibit the self-adhesion of the emulsion seeds under high temperature and high humidity conditions, and make the coating have good compatibility with the modified polyacrylate water-based coating B, so that the two coatings can have good bonding strength, and there will be no separation and peeling problems when the cup is filled with hot water. During the heat sealing process of the cardboard, the seed structure is softer, making the entire coating easy to melt and have good fluidity, thus having good heat sealing performance. The regular linear structure of the ethylene polymerization block in the monomer makes the polymers in the film closer together, and has good water and oil resistance.
[0049] Modified polyacrylate water-based coating B is modified by adding octadecyl acrylate. The hydrophobic alkyl side chains can make the coating surface have good hydrophobicity. Under high temperature and high humidity, the alkyl side chains will not absorb water vapor and cause adhesion between the two cardboards. It contains the same polymerization monomer as the water-based coating B, so that the two coatings have good compatibility.
[0050] Please continue reading Figure 4 , different from the above-mentioned embodiment, the preparation method in this embodiment further includes step S400, drying.
[0051] In this step, five-stage hot air oven drying can be used, and the drying temperatures are 110 / 120 / 130 / 110 / 100°C respectively; the cold cylinder temperature during winding is controlled at about 40°C. The temperature of the paperboard out of the machine is controlled within 45°C to prevent the paper roll from sticking due to excessive winding temperature.
[0052] The method for preparing food cardboard in the embodiment of the present application is to apply the layer-on-layer structural characteristics of two different functional coatings, so that the paper has a lower heat-sealing bonding temperature and will not be damp or heated and sticky, so that the coated food cardboard has a wide application space in the field of food packaging (disposable paper cups, milk tea cups, noodle bowls, etc.). The coated heat-sealed paper has a heat-sealing temperature of 125℃-150℃, 30min COBB≤10g / m2, and an oil-proof grade of 5. The adhesion result after being placed in a constant temperature and humidity chamber at 70℃ and 70% humidity for 24 hours is 2-4 levels for the front and 1-2 levels for the back. In addition, a hot coffee penetration experiment was carried out, and there was no peeling phenomenon on the coated surface (front) after 30 minutes. The two coatings have good compatibility. The specific test results and detection are shown in the following table.
[0053]
[0054]
[0055] The adhesion test standards are shown in the following table.
[0056] Adhesion Rating Almost non-stick (can fall off by itself with a little external force) 1 Slightly sticky but not sticky 2 It feels sticky but basically does not lint when pulled apart 3 The feeling of stickiness is heavy, and the edges of the round cakes are fuzzy, accounting for less than 20% of the area (originally serious) 4 The area of the raised hair accounts for 20% - 40% of the round cake area 5 The area of the raised hair accounts for 40% - 60% of the round cake area 6 The area of the raised hair accounts for 60% - 80% of the round cake area 7 The raised area accounts for more than 80% of the round cake area 8 Sticks together like glue, hard to pull apart 9
[0057] The food paperboard in the embodiment of the present application has developed two functional water-based coatings according to the requirements of the barrier performance and processing performance of the paper cup, and adopts a layer-on-layer coating structure design to give the paper cup good barrier performance. The COBB value of 30 minutes can be controlled within 10g / m2, the Kit value is 5, and there is no leakage after filling the cup with coffee for 30 minutes. The cupping temperature of the paperboard can be controlled at 330-380℃, the paperboard is not easy to stick under high temperature and high humidity, and the cup is pulled out smoothly after being made. The problem that a single coating cannot balance heat sealing and adhesion is solved.
[0058] The above descriptions are only some embodiments of the present application, and do not limit the protection scope of the present application. Any equivalent device or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A method for preparing food cardboard, It is characterized in that The preparation method comprises: Provide base paper; Applying a modified polyacrylate water-based coating A on the base paper to form a heat-sealing functional layer; wherein the modified polyacrylate water-based coating A is a polymer emulsion with a core-shell structure; A modified polyacrylate water-based coating B is coated on the heat-sealing functional layer to form an anti-blocking layer.
2. The preparation method according to claim 1, It is characterized in that The core of the modified polyacrylate water-based coating A is a polymer of ethylene-butyl acrylate, and the polymerized monomers of the shell structure are ethylene, butyl acrylate and methyl acrylate.
3. The preparation method according to claim 2, It is characterized in that In the ethylene-butyl acrylate polymer, the ratio of ethylene to butyl acrylate is 4-6:6-4; in the polymer monomer of the shell structure, the ratio of ethylene, butyl acrylate and methyl acrylate is 3:5:
2.
4. The preparation method according to claim 1, It is characterized in that The modified polyacrylate water-based coating B is formed by polymerization of methyl methacrylate and butyl acrylate.
5. The preparation method according to claim 4, It is characterized in that The ratio of the methyl methacrylate to the butyl acrylate is 7:
3.
6. The preparation method according to claim 4, It is characterized in that The modified polyacrylate water-based coating B also includes octadecyl acrylate, and the added amount of octadecyl acrylate is 5-8% of the total amount of the methyl methacrylate and the butyl acrylate.
7. The preparation method according to claim 4, It is characterized in that The coating amount of the modified polyacrylate water-based coating A is 8-10 g / m2, and the coating amount of the modified polyacrylate water-based coating B is 0.5-2 g / m2.
8. The preparation method according to claim 7, It is characterized in that The thickness of the heat-sealing functional layer is 8-10 um; the thickness of the anti-adhesion layer is 0.5-2 um.
9. The preparation method according to claim 1, It is characterized in that The preparation method also includes a drying process, wherein the drying process adopts five-stage hot air oven drying, and the drying temperatures are 110 / 120 / 130 / 110 / 100° C. respectively.
10. A food cardboard, It is characterized in that The food card paper is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Oil-proof and water-proof acrylic core-shell emulsion for heat sealing and preparation method of oil-proof and water-proof acrylic core-shell emulsion
CN115386045A
Lid member, and manufacturing method for the same
JP2015131659A
Lid material
JP2019014493A
Coating agent for paper, coated paper using the coating agent for paper, bonded body, and packaging material for food products
JP2023094001A
Heat sealable substrate and a process for making the same
US20120302660A1