Improvement method of silty soil in yellow flooding area, roadbed material and application
By mixing the yellow flood silt soil with the photocured aqueous emulsion and the electrolyte sustained release carrier, and energizing during the compaction process, the problem of poor curing strength and water stability of the silt soil is solved, and high intensity and high water stability are achieved The improved soil is suitable for road construction.
Patent Information
- Application Number
- CN202411510224.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to effectively improve the curing strength and water stability of silt soil in yellow flood areas, resulting in limited application in road construction.
By mixing the yellow flood silt with the photocured aqueous emulsion and the electrolyte sustained release carrier, embedded in the cathode and anode, and energizing during the compaction process, the adhesiveness of the silt is improved by using electroosmotic action and chemical reactions during the curing process. and pore structure, thereby improving its curing strength and water stability.
It significantly improves the curing strength and water stability of the silt soil, and forms improved soil with high compressive strength and wear resistance, which is suitable for simple pavement and retaining wall construction.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of silt improvement, and more specifically, to a method for improving silt in the Yellow River flooding area, a roadbed material and an application thereof. Background Art
[0002] Eastern Henan, northern Anhui, northern Jiangsu, and southwestern Shandong belong to the Yellow River flooding area, where a large amount of Yellow River silt has been deposited. Silt has special engineering properties. Generally, more than 70% of the particles are silt and fine sand particles. The specific surface area is not large, the capillary phenomenon is prominent, and it has pseudoplastic characteristics. Silt of different origins has different physical and mechanical properties, poor structural properties, and is very easy to liquefy under dynamic loads. Due to its special physical and mechanical properties, the stability of silt in road engineering has always been a difficult problem to solve.
[0003] At present, there is no effective solution for the low liquid limit sand-containing silt in the Yellow River alluvial plain. There are several ways to solidify silt: Mechanical method: Through compaction technology, the pore volume of the soil can be reduced and the water content can be kept at a fixed level. Although the mechanical method does not require any other substances, it has a poor solidification effect on silt with poor plasticity. Physical method: The physical method mainly adds substances such as asphalt or tar to reduce the water absorption of soil particles and improve the water stability of the soil through the wrapping and adhesion between particles. The asphalt used in the physical method is generally hot asphalt, which needs to be heated, or some room temperature asphalt, such as emulsified asphalt or foamed asphalt, which needs to be emulsified and foamed, which increases the processing cost. Tar is used as an adhesive. Tar itself is a carcinogen and is not environmentally friendly. Chemical method: Inorganic gelling materials and curing agents are more often used to stabilize silt, and each has its own limitations. Silt is almost entirely composed of primary mineral powder particles, with poor plasticity, less active SiO2 and Al2O3 components, poor grading, and less solidified condensate generated by the reaction of lime and soil, resulting in low initial and later strength of ash soil and poor water and frost resistance. Due to poor grading, the filling and bonding of cement cannot be fully exerted; and there are few clay particles in silt, and the amount of dissolved active components is small, so the cement soil system stimulates the soil to generate less hydrated calcium silicate or calcium aluminum silicate cement, so the bonding effect on the soil is poor, and the strength improvement is not obvious; soil stabilizer is an emerging soil solidification method. It is a geocomposite material with excellent performance. It is a material prepared from a variety of inorganic and organic materials and is specially used for soil reinforcement. After mixing with soil, it produces a series of physical and chemical reactions to transform loose soil into dense cementitious materials. However, each stabilizer has its own scope of application. Some soil stabilizers can only meet some single performance indicators and cannot improve the comprehensive performance in many aspects. Some soil stabilizers are often only suitable for certain types of soil, but have little stabilizing effect on other types of soil. Therefore, how to improve the road performance of silty soil and realize the widespread application of low liquid limit silt in road construction is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present application is provided to solve the above defects existing in the prior art. A method for improving silt soil in the Yellow River flooding area, a roadbed material and application are needed, which can greatly improve the solidification strength and water stability of silt soil, and solve the problems that the existing low liquid limit sand-containing silt soil has poor performance after improvement, poor water stability during application, and low mechanical properties.
[0005] In a first aspect of the present application, a method for improving silt soil in the Yellow River flooding area is provided, the improvement method comprising: mixing silt soil in the Yellow River flooding area, a light-cured aqueous emulsion and an electrolyte slow-release carrier to obtain reconstituted soil; embedding a cathode and an anode in the reconstituted soil, and compacting the reconstituted soil, and during the compaction process, the cathode and the anode extending out of the reconstituted soil are respectively connected to an external power supply, and the cathode and the anode are energized by the external power supply; after compaction and molding, disconnecting the cathode and the anode from the external power supply, connecting the cathode and the anode extending out of the reconstituted soil through a wire, and curing the reconstituted soil to obtain improved soil.
[0006] A second aspect of the present application provides a roadbed material, which includes improved soil obtained by the improvement method described in any embodiment of the present application, wherein a cathode and an anode are embedded in the improved soil.
[0007] The third aspect of the present application provides an application of the roadbed material described in any embodiment of the present application in laying roadbed and / or retaining wall.
[0008] The various embodiments of the present application provide a method for improving silt soil in the Yellow River flooding area, a roadbed material and an application. During the improvement process, a light-cured aqueous emulsion and an electrolyte slow-release carrier are added to the silt soil to make the discrete particles of the silt soil adhere to each other, and by implanting a cathode and an anode in the soil body, the electrolyte ions uniformly distributed in the silt soil migrate in the soil body under the action of electroosmosis, thereby increasing the drainage volume during the pressing process; and during the maintenance process, the electrolyte on the electrolyte slow-release carrier continuously generates hydrated calcium silicate in the soil body, cements the clay particles, optimizes the pore structure of the soil body, thereby improving the strength of the soil body and increasing the volume chemical reduction. Therefore, the improvement method of the present application is superior to the existing compaction method and the curing effect of inorganic cementitious materials. The improved soil after improvement in the present application has the advantages of high strength, large water stability coefficient and excellent wear resistance, and can be widely used in simple road paving and retaining wall construction. DETAILED DESCRIPTION
[0009] In order to make those skilled in the art better understand the technical scheme of the present invention, the present invention is described in detail below in conjunction with specific embodiments. The experimental methods for which specific conditions are not indicated in the following examples are usually carried out under normal conditions or according to the conditions recommended by the manufacturer. The test materials used in the following examples, unless otherwise specified, are purchased from conventional biochemical reagent stores. Unless otherwise specified, percentages and parts are calculated by weight. Unless otherwise defined, all professional and scientific terms used in the text have the same meaning as those familiar to those skilled in the art. In addition, any method and material similar to or equal to the recorded content can all be applied to the present invention. The preferred implementation methods and materials described in the text are only for demonstration purposes.
[0010] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0011] According to an embodiment of the present application, a method for improving silt in the Yellow River flooding area is provided, and the improvement method comprises: mixing silt in the Yellow River flooding area, a light-cured aqueous emulsion and an electrolyte slow-release carrier to obtain reconstituted soil; embedding a cathode and an anode in the reconstituted soil, and compacting the reconstituted soil, and during the compaction process, the parts of the cathode and the anode extending out of the reconstituted soil are respectively connected to an external power supply, and the cathode and the anode are energized by the external power supply; after compaction and molding, disconnecting the cathode and the anode from the external power supply, respectively, connecting the parts of the cathode and the anode extending out of the reconstituted soil through a wire, and curing the reconstituted soil to obtain improved soil.
[0012] On the one hand, the light-curing water-based emulsion can connect the discrete particles in the bonding silt to ensure the initial forming and initial strength of the silt. On the other hand, during the curing process, under the action of ultraviolet light, it continues to cross-link and cure, further improving the curing strength of the silt.
[0013] The electrolyte slow-release carrier is evenly dispersed in the silt. During the compaction process, current is applied between the anode and the cathode to migrate the electrolyte ions in the soil, thinning the double electrical layer of the silt particles, thereby reducing the adsorbed bound water, increasing the amount of free water, and improving drainage. During the curing process, the electrolyte continuously generates hydration products in the soil, such as calcium aluminate, which cements the clay particles and fills part of the soil pores, further improving water stability and mechanical properties.
[0014] Therefore, improvements are made to the silt in the Yellow River flooding area, which has poor structure, easy liquefaction and pseudoplasticity. The improved soil has high strength, large water stability coefficient and good wear resistance.
[0015] The silt described in the present application is a low liquid limit sand-containing silt. In some embodiments, the mass of particles with a particle size greater than 0.075 mm in the silt is less than or equal to 50% of the total mass of the silt. In some embodiments, the silt plasticity index IP≤10. In some embodiments, the silt includes but is not limited to the impact soil of the Yellow River Delta. The improvement method of the present application has a good improvement effect on the low liquid limit silt in the Yellow River flooding area.
[0016] In some embodiments, the powdered soil is dried or not dried before being mixed with the light-curable aqueous emulsion and the electrolyte slow-release carrier. In the actual construction process, it is not necessary to dry it. In some experimental processes, it may be preferred to dry it first.
[0017] In some embodiments, water is added during the mixing of silt, light-cured aqueous emulsion and electrolyte. The amount of water added is calculated by subtracting the amount of water in the light-cured aqueous emulsion from the optimum water content, and the optimum water content is obtained by a compaction test of the soil. According to the T0804-1994 standard in JTG E50-2009 "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering", a compaction test is performed on the silt to determine the optimum water content of the silt.
[0018] In some embodiments, the mass ratio of silt, light-cured aqueous emulsion and electrolyte sustained-release carrier is (75-85): (5-8): (20-30). Preferably, the mass ratio of silt, light-cured aqueous emulsion and electrolyte sustained-release carrier is (80-85): (5-6): (23-27).
[0019] In some embodiments, the photocurable aqueous emulsion includes the following components in parts by weight: 50-60 parts of aqueous photocurable emulsion, 1-10 parts of reactive diluent, and 3-6 parts of photoinitiator. As needed, the weight of the aqueous photocurable emulsion can be various, such as 50-58 parts, 50-55 parts, 50-53 parts, 52-60 parts, 55-60 parts, 58-60 parts, etc. As needed, the weight of the reactive diluent can be various, such as 3-10 parts, 5-10, 8-10 parts, 1-4 parts, 1-6 parts, or 1-8 parts, etc. As needed, the weight of the initiator can be various, such as 3-5 parts, 3-4 parts, etc.
[0020] In some embodiments, the aqueous photocurable emulsion is selected from one of polyester acrylate emulsion, polyurethane acrylate emulsion, and epoxy acrylate emulsion; preferably, the aqueous photocurable emulsion is polyurethane acrylate emulsion.
[0021] In some embodiments, the photoinitiator is selected from at least one of TPO, 907 (C13H17NO2S), 184 (1-hydroxycyclohexyl phenyl ketone), 1173 (HMPP), and BP. Preferably, the photoinitiator includes 184 and 1173, and the mass ratio of 1173 to 184 is 1: (1-1.5). When two different photoinitiators are compounded, the absorption wave number range of the initiation system is widened, and the ultraviolet light source is more effectively utilized. The compounded photoinitiator can improve the photoinitiation efficiency to a certain extent.
[0022] Reactive diluents can cross-link with water-based photocurable emulsions, which can reduce resin viscosity and ensure a high cross-linking density. Photoinitiators are key components in photocuring systems. They play a decisive role in the curing speed of photocurable materials and the final realization of film-forming properties. Photoinitiators are substances that can absorb ultraviolet radiation energy, undergo optical changes after excitation, and generate free radicals or cations with the ability to initiate polymerization. Reasonable selection and matching of photoinitiators is an important step in completing photocuring.
[0023] In some embodiments, the reactive diluent is selected from a monofunctional reactive diluent, a bifunctional reactive diluent, and a multifunctional reactive diluent; In some embodiments, the monofunctional reactive diluent includes but is not limited to n-butyl acrylate, isooctyl acrylate, isodecyl acrylate, and lauryl acrylate; the bifunctional reactive diluent includes but is not limited to ethylene glycol diacrylate or propylene glycol diacrylate; the multifunctional reactive diluent includes but is not limited to pentaerythritol triacrylate, trimethylolpropane triacrylate or ethoxytrimethylolpropane triacrylate; preferably, the reactive diluent is selected from one or more of hydroxyethyl methacrylate, hydroxypropyl methacrylate, allyl glycidyl ether, octyl glycidyl ether, butyl glycidyl ether, 1,4-butanediol diglycidyl ether, tetrahydrofurfuryl methacrylate, 1,6-hexanediol diglycidyl ether, and polypropylene glycol diglycidyl ether.
[0024] In some embodiments, the electrolyte sustained-release carrier comprises a porous carrier loaded with electrolytes and a cellulose gel coating the porous carrier.
[0025] In some embodiments, the porous carrier includes one or more of ceramsite, diatomaceous earth, volcanic stone, zeolite, expanded vermiculite, and expanded perlite; the electrolyte is selected from one or more of magnesium chloride, calcium chloride, and sodium bicarbonate. Preferably, the electrolyte includes magnesium chloride and calcium chloride, and the mass ratio of magnesium chloride to calcium chloride is 1: (1-10). Preferably, the electrolyte includes sodium bicarbonate and calcium chloride, and the mass ratio of sodium bicarbonate to calcium chloride is 1: (5-10).
[0026] In some embodiments, the particle size of the porous carrier is 1-10 mm, and the porosity of the porous carrier is 48-55%.
[0027] In some embodiments, the preparation method of the electrolyte sustained-release carrier includes: adding the porous carrier to an electrolyte solution with a concentration of 5-20%wt and shaking it, then drying the porous carrier loaded with electrolyte and putting it into the hydrogel, mixing evenly, and dehydrating it to obtain the result.
[0028] In some embodiments, the hydrogel comprises one or more of methylcellulose gel, cellulose acetate gel, carboxymethylcellulose gel, hydroxypropylcellulose gel, hypromellose gel, and ethylcellulose gel.
[0029] In some embodiments, the current of the cathode and the anode supplied by the external power supply during compaction is 0.50-5.00A / m 2 , the voltage is less than 24V. For example, 12V, etc. The remolded soil is injected into the mold, and the cathode and anode are buried, and a portion of the cathode and anode are leaked, even if a portion of the cathode and anode are penetrated, for connecting an external power supply, so that current is applied to the cathode and anode, so that the electrolyte ions migrate in the soil, and the double electric layer of the silt particles becomes thinner, thereby reducing the adsorbed bound water, increasing the amount of free water, and improving the drainage.
[0030] In some embodiments, after compaction and molding, the mixture is cured for 7-10 days at 25±2°C and relative humidity ≥95%. Since the cathode and the anode form a primary battery through the wire, under the action of the potential difference, the electrolyte on the electrolyte slow-release carrier is continuously released, migrates in the soil, and continuously generates calcium aluminate, filling part of the soil pores, further improving the water stability and mechanical properties. The present application has no special restrictions on the curing method.
[0031] In some embodiments, the anode and cathode can be selected from metal electrodes or graphite electrodes, respectively.
[0032] According to an embodiment of the present application, a roadbed material is also provided, and the roadbed material includes improved soil obtained by the improvement method described in any embodiment of the present application.
[0033] According to an embodiment of the present application, there is also provided a use of the roadbed material described in any embodiment of the present application in laying a roadbed and / or a retaining wall.
[0034] Example 1 The powdered soil, the light-cured aqueous emulsion, the electrolyte slow-release carrier and the added water in a mass ratio of 75:5:23:1 were mixed to obtain the remolded soil. The mixed remolded soil was injected into a mold and embedded with the cathode and the anode. The specimen was formed into a rectangular block according to a compaction degree of 95%, and one end of the cathode and the anode passed through the rectangular block. During the compaction process, an external power supply was connected between the cathode and the anode, and the current was controlled to be 1.5A / m 2 , the voltage is 12V; after the molded specimen is formed, the cathode and the anode are connected by a wire and placed in a curing room for 7 days (25±2℃, relative humidity ≥95%) to obtain improved soil.
[0035] Among them, the silt is collected from the alluvial soil in the Yellow River Delta; In parts by weight, the photocurable aqueous emulsion comprises 50 parts of polyurethane acrylate emulsion, 2 parts of hydroxyethyl methacrylate, 5 parts of tetrahydrofurfuryl methacrylate, and 3 parts of photoinitiator (1173 and 184 in a mass ratio of 1:1); The electrolyte sustained-release carrier is prepared by the following method: adding ceramsite with a particle size of 5-8 mm into a calcium chloride solution with a concentration of 5-20%wt to shake, then drying the ceramsite loaded with calcium chloride and adding it into methylcellulose gel, mixing evenly, and dehydrating to obtain the electrolyte sustained-release carrier.
[0036] Measurement results: According to JTG E50-2009 "Test Code for Inorganic Binder Stabilized Materials for Highway Engineering", unconfined compressive strength test and water stability test were carried out, and the measured 7d unconfined compressive strength was 1.075MPa, 28d unconfined compressive strength was 1.241MPa, and the water stability coefficient was 0.775.
[0037] Example 2 The powdered soil, the light-cured aqueous emulsion, the electrolyte slow-release carrier and the added water in a mass ratio of 80:6:20:3 were mixed to obtain the remolded soil. The mixed remolded soil was injected into a mold and embedded with the cathode and the anode. The specimen was formed into a rectangular block according to a compaction degree of 95%, and one end of the cathode and the anode passed through the rectangular block. During the compaction process, an external power supply was connected between the cathode and the anode, and the current was controlled to be 1.5A / m 2 , the voltage is 12V; after the molded specimen is formed, the cathode and the anode are connected by a wire and placed in a curing room for 7 days (25±2℃, relative humidity ≥95%) to obtain improved soil.
[0038] Among them, the silt is collected from the alluvial soil in the Yellow River Delta; The photocurable aqueous emulsion comprises 60 parts of polyurethane acrylate emulsion, 8 parts of hydroxypropyl methacrylate, and 5 parts of photoinitiator (1173 and 184 in a mass ratio of 1:1.2) in a mixture; The electrolyte sustained-release carrier is prepared by the following method: adding ceramsite with a particle size of 5-8 mm into a calcium chloride solution with a concentration of 5-20%wt to shake, then drying the ceramsite loaded with calcium chloride and adding it into methylcellulose gel, mixing evenly, and dehydrating to obtain the electrolyte sustained-release carrier.
[0039] Measurement results: According to JTG E50-2009 "Test Code for Inorganic Binder Stabilized Materials for Highway Engineering", unconfined compressive strength test and water stability test were carried out, and the measured 7d unconfined compressive strength was 1.091MPa, 28d unconfined compressive strength was 1.218MPa, and the water stability coefficient was 0.768.
[0040] Example 3 The powdered soil, the light-cured aqueous emulsion, the electrolyte slow-release carrier and the added water in a mass ratio of 85:8:27:4 were mixed to obtain the remolded soil. The mixed remolded soil was injected into a mold and embedded with the cathode and the anode. The specimen was formed into a rectangular block according to a compaction degree of 95%, and one end of the cathode and the anode passed through the rectangular block. During the compaction process, an external power supply was connected between the cathode and the anode, and the current was controlled to be 1.5A / m 2 , the voltage is 12V; after the molded specimen is formed, the cathode and the anode are connected by a wire and placed in a curing room for 7 days (25±2℃, relative humidity ≥95%) to obtain improved soil.
[0041] Among them, the silt is collected from the alluvial soil in the Yellow River Delta; The photocurable aqueous emulsion comprises, by weight, 50 parts of polyurethane acrylate emulsion, 4 parts of 1,6-hexanediol diglycidyl ether, 3 parts of tetrahydrofurfuryl methacrylate, and 3 parts of photoinitiator (1173 and 184 in a weight ratio of 1:1.5); The electrolyte sustained-release carrier is prepared by the following method: adding ceramsite with a particle size of 5-8 mm into a calcium chloride solution with a concentration of 5-20%wt to shake, then drying the ceramsite loaded with calcium chloride and adding it into methylcellulose gel, mixing evenly, and dehydrating to obtain the electrolyte sustained-release carrier.
[0042] Measurement results: According to JTG E50-2009 "Test Code for Inorganic Binder Stabilized Materials for Highway Engineering", unconfined compressive strength test and water stability test were carried out, and the measured 7d unconfined compressive strength was 1.215MPa, 28d unconfined compressive strength was 1.521MPa, and the water stability coefficient was 0.802.
[0043] Example 4 The powdered soil, the light-cured aqueous emulsion and the electrolyte slow-release carrier in a mass ratio of 85:8:20:3.5 were mixed to obtain the remolded soil. The mixed remolded soil was injected into a mold and embedded with a cathode and an anode. The specimen was formed into a rectangular block at a compaction degree of 95%, and one end of the cathode and the anode passed through the rectangular block. During the compaction process, an external power supply was connected between the cathode and the anode, and the current was controlled to be 1.5A / m 2 , the voltage is 12V; after the molded specimen is formed, the cathode and the anode are connected by a wire and placed in a curing room for 7 days (25±2℃, relative humidity ≥95%) to obtain improved soil.
[0044] Among them, the silt is collected from the alluvial soil in the Yellow River Delta; The photocurable aqueous emulsion comprises, by weight, 58 parts of polyurethane acrylate emulsion, 6 parts of polypropylene glycol diglycidyl ether, 1 part of allyl glycidyl ether, and 4 parts of photoinitiator (1173 and 184 in a weight ratio of 1:1.2); The electrolyte sustained-release carrier is prepared by the following method: adding ceramsite with a particle size of 5-8 mm into a calcium chloride solution with a concentration of 5-20%wt to shake, then drying the ceramsite loaded with calcium chloride and adding it into methylcellulose gel, mixing evenly, and dehydrating to obtain the electrolyte sustained-release carrier.
[0045] Measurement results: According to JTG E50-2009 "Test Code for Inorganic Binder Stabilized Materials for Highway Engineering", unconfined compressive strength test and water stability test were carried out, and the measured 7d unconfined compressive strength was 1.247MPa, 28d unconfined compressive strength was 1.4881MPa, and the water stability coefficient was 0.796.
[0046] Example 5 The remolded soil was prepared by mixing the silt, light-cured aqueous emulsion, electrolyte slow-release carrier and added water in a mass ratio of 80:5:23:2.5. The mixed remolded soil was injected into a mold and embedded with a cathode and an anode. The specimen was formed into a rectangular block at a compaction degree of 95%, and one end of the cathode and the anode passed through the rectangular block. During the compaction process, an external power supply was connected between the cathode and the anode, and the current was controlled to be 1.5A / m 2 , the voltage is 12V; after the molded specimen is formed, the cathode and the anode are connected by a wire and placed in a curing room for 7 days (25±2℃, relative humidity ≥95%) to obtain improved soil.
[0047] Among them, the silt is collected from the alluvial soil in the Yellow River Delta; The photocurable aqueous emulsion comprises 52 parts of polyurethane acrylate emulsion, 5 parts of tetrahydrofurfuryl methacrylate, and 5 parts of photoinitiator (1173 and 184 in a mass ratio of 1:1) in a mixture; The electrolyte sustained-release carrier is prepared by the following method: adding ceramsite with a particle size of 5-8 mm into a calcium chloride solution with a concentration of 5-20%wt to shake, then drying the ceramsite loaded with calcium chloride and adding it into methylcellulose gel, mixing evenly, and dehydrating to obtain the electrolyte sustained-release carrier.
[0048] Measurement results: According to JTG E50-2009 "Test Code for Inorganic Binder Stabilized Materials for Highway Engineering", unconfined compressive strength test and water stability test were carried out, and the measured 7d unconfined compressive strength was 1.032MPa, 28d unconfined compressive strength was 1.274MPa, and the water stability coefficient was 0.782.
[0049] The silt solidification methods of Examples 1-5 can significantly increase the solidification strength of the silt, and the strength is suitable for the base and subbase strength standards of various highways, and the strength is gradually enhanced.
[0050] The improved soil obtained in Examples 1-5 did not liquefy in the compressive strength test, indicating that the improved soil has good water stability.
[0051] Comparative Example 1 The same as Example 3, except that the photocurable aqueous emulsion is replaced by SBS latex.
[0052] Measurement results: According to JTG E50-2009 "Test Code for Inorganic Binder Stabilized Materials for Highway Engineering", unconfined compressive strength test and water stability test were carried out, and the measured 7d unconfined compressive strength was 0.994MPa, 28d unconfined compressive strength was 1.274MPa, and the water stability coefficient was 0.787.
[0053] Comparative Example 2 Same as Example 3, except that the light-cured aqueous emulsion is replaced with silicate cement. Test results: According to JTG E50-2009 "Testing Procedure for Stabilized Materials of Inorganic Binders for Highway Engineering", the unconfined compressive strength test and water stability test were conducted, and the 7d unconfined compressive strength was 0.813MPa, the 28d unconfined compressive strength was 1.119MPa, and the water stability coefficient was 0.742.
[0054] Comparative Example 3 The same as Example 4, except that no electrolyte slow-release carrier is added. Measurement results: According to JTG E50-2009 "Test Procedure for Stabilized Materials of Inorganic Binders for Highway Engineering", the unconfined compressive strength test and water stability test were carried out, and the unconfined compressive strength at 7d was 0.905MPa, the unconfined compressive strength at 28d was 1.163MPa, and the water stability coefficient was 0.759.
[0055] Comparative Example 4 Same as Example 4, except that the electrolyte is calcium chloride. Test results: According to JTG E50-2009 "Testing Procedure for Inorganic Binder Stabilized Materials for Highway Engineering", the unconfined compressive strength test and water stability test were conducted, and the unconfined compressive strength at 7d was 1.107MPa, the unconfined compressive strength at 28d was 1.254MPa, and the water stability coefficient was 0.781.
[0056] Comparative Examples 1 and 2 show that the light-cured aqueous emulsion can improve the compressive strength and water stability of the improved soil. Comparative Examples 3 and 4 show that the compressive strength and water stability of the improved soil are reduced when calcium chloride is used alone as an electrolyte or when no electrolyte slow-release carrier is added.
[0057] In addition, although exemplary embodiments have been described herein, the scope includes any and all embodiments based on the present application with equivalent elements, modifications, omissions, combinations (e.g., various embodiments intersecting schemes), adaptations or changes. The elements in the claims are to be interpreted broadly based on the language adopted in the claims, and are not limited to the examples described in this specification or during the practice of this application, and the examples are to be interpreted as non-exclusive. Therefore, this specification and examples are intended to be considered as examples only, and the true scope and spirit are indicated by the following claims and the full scope of their equivalents.
[0058] The above description is intended to be illustrative rather than restrictive. For example, the above examples (or one or more schemes thereof) may be used in combination with each other. For example, a person of ordinary skill in the art may use other embodiments when reading the above description. In addition, in the above-mentioned specific embodiments, various features may be grouped together to simplify the present application. This should not be interpreted as an intention that a feature of an application that does not require protection is necessary for any claim. On the contrary, the subject matter of the present application may be less than all the features of an embodiment of a particular application. Thus, the following claims are incorporated herein in the specific embodiments as examples or embodiments, wherein each claim is independently a separate embodiment, and it is considered that these embodiments may be combined with each other in various combinations or arrangements. The scope of the present invention should be determined with reference to the appended claims and the full scope of equivalent forms granted by these claims.
[0059] The above embodiments are only exemplary embodiments of the present application and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present application, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.
Claims
1. A method for improving silt sand in the Yellow River flooding area. It is characterized in that The improvement method comprises: mixing silt from the Yellow River flooding area, a light-cured aqueous emulsion and an electrolyte slow-release carrier to obtain remolded soil; Embedding a cathode and an anode in the remolded soil, and compacting the remolded soil, and during the compaction process, portions of the cathode and the anode extending out of the remolded soil are respectively connected to an external power source, and the cathode and the anode are energized by the external power source; After compaction and molding, the cathode and the anode are disconnected from the external power supply respectively, the cathode and the anode portions extending out of the remolded soil are connected through a wire, and the remolded soil is cured to obtain improved soil.
2. The improved method according to claim 1, It is characterized in that The mass of particles with a particle size greater than 0.075 mm in the silt is less than or equal to 50% of the total mass of the silt.
3. The improved method according to claim 1, It is characterized in that The mass ratio of silt, light-cured aqueous emulsion and electrolyte sustained-release carrier is (75-85):(5-8):(20-30).
4. The improved method according to claim 1, It is characterized in that The photocurable aqueous emulsion comprises the following components in parts by weight: 50-60 parts of aqueous photocurable emulsion, 1-10 parts of reactive diluent, and 3-6 parts of photoinitiator.
5. The improved method according to claim 1, It is characterized in that The electrolyte sustained-release carrier comprises a porous carrier loaded with electrolyte and a cellulose gel coating the porous carrier.
6. The improved method according to claim 5, It is characterized in that The porous carrier includes one or more of ceramsite, diatomaceous earth, volcanic stone, zeolite, expanded vermiculite, and expanded perlite; the electrolyte is selected from one or more of magnesium chloride, calcium chloride, and sodium bicarbonate.
7. The improved method according to claim 1, It is characterized in that During the compaction process, the current supplied to the cathode and anode by the external power supply is 0.50-5.00A / m 2 , the voltage is less than 24V.
8. The improved method according to claim 1, It is characterized in that After compaction, cure for 7-10 days at 25±2℃ and relative humidity ≥95%.
9. A roadbed material, It is characterized in that The roadbed material includes improved soil obtained by the improvement method according to any one of claims 1-8.
10. Use of the roadbed material according to claim 9 in laying roadbed and / or retaining wall.