Polishing method of thin-film lithium niobate optical waveguide chip
By using NH4OH and H2O2 polishing liquid and silica protective layer on the optical waveguide chip, combined with wet etching technology, the problems of long polishing, high cost and narrow application range in the existing technology are solved, and the rapid and Low-cost optical waveguide chip polishing improves optical quality and performance stability.
Patent Information
- Application Number
- CN202410981109.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-12-03
AI Technical Summary
The existing optical waveguide chip polishing technology is time-consuming, high cost and narrow in scope, and it has failed to effectively solve the problems of optical signal loss and reflection.
Chemical corrosion polishing is used to use polishing liquid containing NH4OH and H2O2, combined with silica protective layer and wet etching technology, the concentration and temperature of the polishing liquid are controlled to achieve fast and low-cost polishing of the optical waveguide end surface.
Significantly shortens polishing time, reduces costs, broadens the scope of application, improves the optical quality and performance stability of optical waveguide chips, and reduces process losses and environmental impacts.
Smart Images

Figure CN119065060A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thin-film lithium niobate optical waveguide chips, and in particular relates to a polishing method for thin-film lithium niobate optical waveguide chips. Background Art
[0002] Optical waveguide end face polishing refers to the processing of the end face of an optical waveguide (optical fiber or other optical guide material) to ensure the flatness and optical quality of the end face, thereby reducing the loss and reflection of the optical signal. This is a very important step in optical communications and optical sensors. The unpolished optical fiber end face may have an uneven surface, which will cause scattering and absorption of the optical signal during transmission, increasing the loss. Polishing can make the end face smoother, thereby reducing the loss of the optical signal during transmission and improving the transmission efficiency. At the same time, the uneven end face will cause the reflection of the optical signal, and the reflected optical signal will return to the light source end, which may cause interference and signal distortion. The smooth end face after polishing can reduce reflection and maintain the integrity and stability of the optical signal. Therefore, a smooth and flat end face plays a vital role in the performance of optical waveguide devices.
[0003] The polishing scheme currently used is chemical mechanical polishing (CMP), which mainly involves the following steps: (1) Rough polishing: Use coarse abrasives to remove most of the surface unevenness and form a basically flat end face; (2) Medium polishing: Use medium-grained abrasives for further fine grinding to eliminate the traces left by rough polishing; (3) Fine polishing: Use fine-grained abrasives for the final polishing to ensure that the end face reaches a mirror effect; (4) Cleaning: After each step of polishing, it must be thoroughly cleaned to remove grinding residues and avoid contamination of subsequent polishing steps. The entire process of this polishing technology takes a long time (about 1 hour), and the sandpaper needs to be replaced back and forth. The polishing liquid is expensive, and the particles and impurities generated during the polishing process are easy to contaminate the surface of the optical waveguide device. At the same time, CMP requires the size of the optical waveguide device to be large and the shape to be regular for easy clamping. Therefore, the current polishing scheme has a narrow scope of application. Summary of the invention
[0004] The present invention aims to solve at least one of the above technical problems existing in the prior art. To this end, the present invention provides a polishing method for a thin-film lithium niobate optical waveguide chip, which has the advantages of low cost, high efficiency and short time consumption.
[0005] In the first aspect, some embodiments of the present invention provide a method for polishing a thin-film lithium niobate optical waveguide chip, comprising the steps of depositing a protective layer on the surface of the thin-film lithium niobate optical waveguide chip, coating a photoresist, cutting, debonding, and etching and polishing, wherein the polishing liquid for etching and polishing contains NH4OH and H2O2.
[0006] It can be understood that the polishing method of the present invention, by using a polishing liquid containing NH4OH and H2O2 to chemically etch and polish the end face of the thin-film lithium niobate waveguide to obtain a smooth optical waveguide end face, has the advantages of low cost, high efficiency and short time consumption. Specifically:
[0007] In terms of cost, NH4OH and H2O2 solutions are cheap, can process multiple optical chips at the same time, and can be used on a large scale, so the cost is low.
[0008] In terms of efficiency, since the etching and polishing step is wet etching, the rate can be adjusted by controlling the processing temperature, and fine polishing of the end face can be achieved.
[0009] In terms of time consumption, rapid wet polishing can be performed by increasing the etching rate, shortening the polishing time from the current 1 hour to 10 minutes.
[0010] In addition, since the etching and polishing steps are wet etching, there are no requirements for the size and shape of the optical waveguide device and no clamping is required, which greatly broadens the scope of application.
[0011] In combination with the first aspect, in some embodiments of the present invention, the protective layer includes a silicon dioxide protective layer.
[0012] The silicon dioxide protective layer can effectively protect the surface of the lithium niobate thin film optical waveguide chip from mechanical damage and chemical erosion. During the preparation of the optical waveguide chip, it can prevent foreign particles or harmful substances in the solution from directly contacting the chip surface, ensuring the quality and performance stability of the optical waveguide during the preparation process. The silicon dioxide protective layer itself has good flatness and chemical stability, and can provide a uniform and reliable basis for subsequent photoresist coating and etching steps. This helps to ensure that the smoothness and consistency of the end face are maintained during the etching and polishing process, thereby improving the preparation accuracy and performance of the optical waveguide chip. The silicon dioxide material has good compatibility with chemicals commonly used in wet etching, such as NH4OH and H2O2, and will not react adversely with the etching solution or affect its stability. Therefore, it ensures the reliability and efficiency of the etching and polishing process and reduces unnecessary process losses and waste. In general, the application of the silicon dioxide protective layer in the polishing method of lithium niobate optical waveguide chips can not only effectively improve the safety and controllability of the preparation process, but also significantly improve the quality and performance of the final product.
[0013] In combination with the first aspect, in some embodiments of the present invention, the cutting passes through the waveguide.
[0014] It should be noted that the purpose of cutting through the waveguide is to form a waveguide end face at the edge of the chip.
[0015] The cut through the waveguide needs to be as flat as possible to facilitate subsequent chemical solution polishing.
[0016] In combination with the first aspect, in some embodiments of the present invention, the polishing liquid for etching and polishing is an aqueous solution of NH4OH and H2O2.
[0017] The solution composed of NH4OH and H2O2 can effectively chemically corrode the end face of lithium niobate optical waveguide. This corrosion effect enables the removal of uneven or incomplete parts of the surface during the etching and polishing process, thereby obtaining a smoother and more regular optical waveguide end face. During the wet etching process, the NH4OH and H2O2 solutions can control the polishing rate and accuracy by adjusting the concentration, temperature and processing time of the etching solution. In this way, fine polishing of the optical waveguide end face can be achieved, and the optical quality and performance of the optical waveguide can be improved. Furthermore, NH4OH and H2O2 are relatively cheap and easily available chemicals, and their aqueous solutions can be used in batches, which are suitable for large-scale manufacturing and processing of optical waveguide devices. Therefore, compared with other polishing methods, the use of this solution can significantly reduce manufacturing costs. In addition, the by-products produced by the NH4OH and H2O2 solutions during use are relatively small, and the impact on the environment is small, which meets the requirements and standards of green manufacturing. Using NH4OH and H2O2 solutions for etching and polishing can achieve the controllability and stability of the end face quality during the preparation of optical waveguide devices. The operation is simple and suitable for a variety of optical waveguide materials and structures, which improves the versatility and adaptability of the process. Therefore, NH4OH and H2O2 aqueous solutions have significant advantages as etching and polishing liquids in the preparation of lithium niobate optical waveguide devices, which can effectively improve the end face quality, improve manufacturing efficiency, and have high cost-effectiveness and environmental friendliness.
[0018] In combination with the first aspect, in some embodiments of the present invention, the volume percentage of NH4OH in the polishing liquid is 20 vol% to 50 vol%.
[0019] When the concentration of NH4OH is too low, its chemical corrosion effect on lithium niobate is insufficient, which may cause the etching and polishing rate to be too slow, affecting the process efficiency. It may also cause unevenness of the end face during the etching process, and the surface may be uneven or residues may appear. When the concentration of NH4OH is too high, the etching effect is too strong, which may lead to excessive removal of lithium niobate materials, causing damage or distortion of the end face and affecting the optical performance. High-concentration NH4OH solutions may be unstable, making it difficult to control the etching process and results, affecting the repeatability and stability of the process. In addition, high-concentration NH4OH solutions may cause greater hazards and risks to operators and the environment.
[0020] Therefore, in order to ensure the effect and stability of etching and polishing, as well as the controllability and safety of the process, the volume percentage of NH4OH should be controlled in the range of 20vol% to 50vol%. Solutions within this range can provide appropriate etching rate and surface quality while maintaining good operability and environmental friendliness.
[0021] In combination with the first aspect, in some embodiments of the present invention, the volume percentage of NH4OH in the polishing liquid is 30 vol% to 40 vol%.
[0022] In combination with the first aspect, in some embodiments of the present invention, the volume percentage of NH4OH in the polishing liquid is any value of 30vol%, 31vol%, 32vol%, 33vol%, 34vol%, 35vol%, 36vol%, 37vol%, 38vol%, 39vol%, 40vol% or a range formed by any two of them.
[0023] In combination with the first aspect, in some embodiments of the present invention, the volume percentage of H2O2 in the polishing liquid is 20 vol% to 50 vol%.
[0024] The volume percentage of H2O2 (hydrogen peroxide) is usually controlled within the range of 20 vol% to 50 vol%, because within this concentration range, the H2O2 solution has the most suitable chemical properties and effects for etching and polishing. When the H2O2 concentration is too low, its oxidizing property is not enough to effectively participate in the etching process, resulting in poor polishing effect, and a longer polishing time is required to achieve the required surface quality. It may also lead to insufficient oxidation reaction in the etching solution, and the impurities and unevenness on the surface of lithium niobate cannot be completely removed, affecting the optical properties of the end face. When the H2O2 concentration is too high, its strong oxidizing property may cause excessive etching of the lithium niobate material, making the end face surface rough or cracked, affecting the performance and reliability of the optical waveguide device. High-concentration H2O2 solutions may be unstable during use, making it difficult to control the reaction rate and results during the etching process, affecting the repeatability and stability of the process. In addition, high-concentration H2O2 solutions have high oxidizing properties, which may increase the safety risks of operators and the environment, and require stricter operating controls and protective measures.
[0025] Therefore, in order to ensure the effect and stability of the etching and polishing process, as well as the controllability and safety of the process, the volume percentage of H2O2 should be controlled within the range of 20vol% to 50vol%. Solutions within this range can provide appropriate oxidation and etching rates while maintaining good operability and environmental friendliness.
[0026] In combination with the first aspect, in some embodiments of the present invention, the volume percentage of H2O2 in the polishing liquid is any value of 30vol%, 31vol%, 32vol%, 33vol%, 34vol%, 35vol%, 36vol%, 37vol%, 38vol%, 39vol%, 40vol% or a range formed by any two of them.
[0027] In combination with the first aspect, in some embodiments of the present invention, the volume ratio of NH4OH, H2O2 and water in the polishing liquid is 2:2:1.
[0028] In combination with the first aspect, in some embodiments of the present invention, the temperature of etching and polishing is 25°C to 100°C.
[0029] It should be noted that too low a temperature will reduce the rate of chemical reactions in the etching solution, resulting in a slow etching process and prolonged polishing time. The reactivity of the etching solution deteriorates at low temperatures, which may cause insufficient reaction between NH4OH and H2O2 in the etching solution, affecting the uniformity and quality of etching, and making the reactivity difficult to control. High temperatures may cause the decomposition or instability of the chemical components in the etching solution, causing the etching solution to lose its original activity and effect. High temperatures may also cause surface denaturation or thermal damage to the lithium niobate material, deteriorating the surface quality of the optical waveguide, and even causing deformation or cracks in the material.
[0030] Therefore, in order to ensure the effect and stability of the etching and polishing process, as well as the controllability and safety of the process, the etching and polishing temperature should be controlled within the range of 25°C to 100°C. Within this range, the etching rate, reaction uniformity and material stability can be balanced, thereby ensuring the quality and performance of the optical waveguide device preparation.
[0031] In combination with the first aspect, in some embodiments of the present invention, the temperature of etching and polishing is 50°C to 95°C.
[0032] In combination with the first aspect, in some embodiments of the present invention, the temperature of etching and polishing is 60°C to 85°C.
[0033] In combination with the first aspect, in some embodiments of the present invention, the etching and polishing time is 5 minutes to 30 minutes.
[0034] Time control during the etching and polishing process is very important for ensuring the etching depth and surface quality. Normally, the etching and polishing time is controlled within the range of 5 minutes to 30 minutes, which can effectively control the etching depth and ensure the smoothness of the surface. Too short a time may result in insufficient etching depth, and the impurities and unevenness on the surface cannot be completely removed, affecting the optical performance and quality of the end face. Insufficient etching time may also cause the end face surface to be uneven or residual unetched areas, affecting the final performance of the optical waveguide device. If the time is too long, it will lead to excessive etching of the lithium niobate material, which may deteriorate the surface quality of the end face and even cause damage or deformation of the surface. In addition, too long an etching time will increase the manufacturing cycle and cost, and reduce the efficiency and economy of the process.
[0035] Therefore, in order to ensure the effect and stability of the etching and polishing process, as well as the controllability and economy of the process, the etching and polishing time should be strictly controlled within the range of 5 minutes to 30 minutes. Within this time range, the etching depth and surface smoothness can be effectively controlled, thereby ensuring the quality and performance of the optical waveguide device preparation.
[0036] In combination with the first aspect, in some embodiments of the present invention, the etching and polishing time is 2 minutes to 25 minutes.
[0037] In combination with the first aspect, in some embodiments of the present invention, the polishing method further comprises the step of placing the thin film lithium niobate optical waveguide chip in deionized water to remove residual solution after etching and polishing.
[0038] The NH4OH and H2O2 solutions used in the etching and polishing process may leave a small amount of chemical residue on the surface of the optical waveguide. Placing the chip in deionized water can effectively remove these residues and ensure the cleanliness and purity of the optical waveguide surface. Deionized water has high purity and low ion content, and will not cause secondary contamination or corrosion to the surface of the optical waveguide. This can ensure that the end face of the optical waveguide after etching and polishing maintains good chemical stability and optical properties. Deionized water can effectively reduce the impact of the medium on the performance of the optical waveguide and improve the stability and reliability of the device. This is especially important for optical devices that require long-term stable operation. Incorporating the deionized water cleaning step into the polishing method can improve the entire process flow and ensure the quality and consistency of each step. This helps to improve manufacturing efficiency and reduce defective rates.
[0039] In combination with the first aspect, in some embodiments of the present invention, the polishing method further comprises the step of drying the thin film lithium niobate optical waveguide chip with nitrogen after removing the residual solution.
[0040] Nitrogen drying can effectively remove residual moisture and prevent water spots from being left on the surface of the device. This is particularly important for the optical performance of the optical waveguide, because water spots may cause scattering or loss of light transmission, and can prevent the device from undergoing oxidation reactions in the air, keeping the surface clean and stable. Using nitrogen to dry can also effectively avoid leaving ionic pollutants on the surface, which may affect the electrical properties and long-term stability of the optical waveguide. It is easy to understand that nitrogen drying is a fast and effective step that can quickly dry the surface of the device, shorten the manufacturing cycle, and improve production efficiency. In addition, nitrogen is a harmless and environmentally friendly gas. Using nitrogen to dry avoids the use of organic solvents or other drying methods that may be harmful to the environment, which meets the requirements of green manufacturing. The surface of the optical waveguide chip after drying is clean and free of water spots, and provides a clean and stable foundation for subsequent subsequent processing steps, such as packaging and testing of optical waveguide devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 Flow chart of the polishing process.
[0042] Figure 2 A top view of the polishing process.
[0043] Figure 3 A side view of the polishing process.
[0044] Figure 4 This is the micro-optical morphology of the waveguide end face before the optical waveguide chip is placed in the polishing liquid for etching and polishing in the embodiment.
[0045] Figure 5 This is the micro-light morphology of the waveguide end face after the optical waveguide chip is placed in the polishing liquid for etching and polishing in the embodiment. DETAILED DESCRIPTION
[0046] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0047] In the first aspect, some embodiments of the present invention provide a method for polishing a thin-film lithium niobate optical waveguide chip, comprising the steps of depositing a protective layer on the surface of the thin-film lithium niobate optical waveguide chip, coating a photoresist, cutting, debonding, and etching and polishing, wherein the etching and polishing polishing liquid contains NH4OH and H2O2.
[0048] It can be understood that the polishing method of the present invention, by using a polishing liquid containing NH4OH and H2O2 to chemically etch and polish the end face of the thin-film lithium niobate waveguide to obtain a smooth optical waveguide end face, has the advantages of low cost, high efficiency and short time consumption. Specifically:
[0049] In terms of cost, NH4OH and H2O2 solutions are cheap, can process multiple optical chips at the same time, and can be used on a large scale, so the cost is low.
[0050] In terms of efficiency, since the etching and polishing step is wet etching, the rate can be adjusted by controlling the processing temperature, and fine polishing of the end face can be achieved.
[0051] In terms of time consumption, rapid wet polishing can be performed by increasing the etching rate, shortening the polishing time from the current 1 hour to 10 minutes.
[0052] In addition, since the etching and polishing steps are wet etching, there are no requirements for the size and shape of the optical waveguide device and no clamping is required, which greatly broadens the scope of application.
[0053] According to some embodiments of the present invention, the protective layer comprises a silicon dioxide protective layer.
[0054] The silicon dioxide protective layer can effectively protect the surface of the lithium niobate thin film optical waveguide chip from mechanical damage and chemical erosion. During the preparation of the optical waveguide chip, it can prevent foreign particles or harmful substances in the solution from directly contacting the chip surface, ensuring the quality and performance stability of the optical waveguide during the preparation process. The silicon dioxide protective layer itself has good flatness and chemical stability, and can provide a uniform and reliable basis for subsequent photoresist coating and etching steps. This helps to ensure that the smoothness and consistency of the end face are maintained during the etching and polishing process, thereby improving the preparation accuracy and performance of the optical waveguide chip. The silicon dioxide material has good compatibility with chemicals commonly used in wet etching, such as NH4OH and H2O2, and will not react adversely with the etching solution or affect its stability. Therefore, it ensures the reliability and efficiency of the etching and polishing process and reduces unnecessary process losses and waste. In general, the application of the silicon dioxide protective layer in the polishing method of lithium niobate optical waveguide chips can not only effectively improve the safety and controllability of the preparation process, but also significantly improve the quality and performance of the final product.
[0055] According to some embodiments of the invention, the cutting is through a waveguide.
[0056] The purpose of cutting through the waveguide is to form a waveguide end face at the edge of the chip.
[0057] The cut through the waveguide needs to be as flat as possible to facilitate subsequent chemical solution polishing.
[0058] According to some embodiments of the present invention, the polishing liquid for etching and polishing is an aqueous solution of NH4OH and H2O2.
[0059] The solution composed of NH4OH and H2O2 can effectively chemically corrode the end face of lithium niobate optical waveguide. This corrosion effect enables the removal of uneven or incomplete parts of the surface during the etching and polishing process, thereby obtaining a smoother and more regular optical waveguide end face. During the wet etching process, the NH4OH and H2O2 solutions can control the polishing rate and accuracy by adjusting the concentration, temperature and processing time of the etching solution. In this way, fine polishing of the optical waveguide end face can be achieved, and the optical quality and performance of the optical waveguide can be improved. Furthermore, NH4OH and H2O2 are relatively cheap and easily available chemicals, and their aqueous solutions can be used in batches, which are suitable for large-scale manufacturing and processing of optical waveguide devices. Therefore, compared with other polishing methods, the use of this solution can significantly reduce manufacturing costs. In addition, the by-products produced by the NH4OH and H2O2 solutions during use are relatively small, and the impact on the environment is small, which meets the requirements and standards of green manufacturing. Using NH4OH and H2O2 solutions for etching and polishing can achieve the controllability and stability of the end face quality during the preparation of optical waveguide devices. The operation is simple and suitable for a variety of optical waveguide materials and structures, which improves the versatility and adaptability of the process. Therefore, NH4OH and H2O2 aqueous solutions have significant advantages as etching and polishing liquids in the preparation of lithium niobate optical waveguide devices, which can effectively improve the end face quality, improve manufacturing efficiency, and have high cost-effectiveness and environmental friendliness.
[0060] According to some embodiments of the present invention, in the polishing liquid, the volume percentage of NH4OH is 20 vol% to 50 vol%.
[0061] When the concentration of NH4OH is too low, its chemical corrosion effect on lithium niobate is insufficient, which may cause the etching and polishing rate to be too slow, affecting the process efficiency. It may also cause unevenness of the end face during the etching process, and the surface may be uneven or residues may appear. When the concentration of NH4OH is too high, the etching effect is too strong, which may lead to excessive removal of lithium niobate materials, causing damage or distortion of the end face and affecting the optical performance. High-concentration NH4OH solutions may be unstable, making it difficult to control the etching process and results, affecting the repeatability and stability of the process. In addition, high-concentration NH4OH solutions may cause greater hazards and risks to operators and the environment.
[0062] Therefore, in order to ensure the effect and stability of etching and polishing, as well as the controllability and safety of the process, the volume percentage of NH4OH should be controlled in the range of 20vol% to 50vol%. Solutions within this range can provide appropriate etching rate and surface quality while maintaining good operability and environmental friendliness.
[0063] According to some embodiments of the present invention, in the polishing liquid, the volume percentage of NH4OH is 30 vol% to 40 vol%.
[0064] According to some embodiments of the present invention, in the polishing liquid, the volume percentage of NH4OH is any value of 30vol%, 31vol%, 32vol%, 33vol%, 34vol%, 35vol%, 36vol%, 37vol%, 38vol%, 39vol%, 40vol%, or a range formed by any two of them.
[0065] According to some embodiments of the present invention, in the polishing liquid, the volume percentage of H2O2 is 20 vol% to 50 vol%.
[0066] The volume percentage of H2O2 (hydrogen peroxide) is usually controlled within the range of 20 vol% to 50 vol%, because within this concentration range, the H2O2 solution has the most suitable chemical properties and effects for etching and polishing. When the H2O2 concentration is too low, its oxidizing property is not enough to effectively participate in the etching process, resulting in poor polishing effect, and a longer polishing time is required to achieve the required surface quality. It may also lead to insufficient oxidation reaction in the etching solution, and the impurities and unevenness on the surface of lithium niobate cannot be completely removed, affecting the optical properties of the end face. When the H2O2 concentration is too high, its strong oxidizing property may cause excessive etching of the lithium niobate material, making the end face surface rough or cracked, affecting the performance and reliability of the optical waveguide device. High-concentration H2O2 solutions may be unstable during use, making it difficult to control the reaction rate and results during the etching process, affecting the repeatability and stability of the process. In addition, high-concentration H2O2 solutions have high oxidizing properties, which may increase the safety risks of operators and the environment, and require stricter operating controls and protective measures.
[0067] Therefore, in order to ensure the effect and stability of the etching and polishing process, as well as the controllability and safety of the process, the volume percentage of H2O2 should be controlled within the range of 20vol% to 50vol%. Solutions within this range can provide appropriate oxidation and etching rates while maintaining good operability and environmental friendliness.
[0068] According to some embodiments of the present invention, in the polishing liquid, the volume percentage of H2O2 is any value of 30vol%, 31vol%, 32vol%, 33vol%, 34vol%, 35vol%, 36vol%, 37vol%, 38vol%, 39vol%, 40vol% or a range formed by any two of them.
[0069] According to some embodiments of the present invention, in the polishing liquid, the volume ratio of NH4OH, H2O2 and water is 2:2:1.
[0070] According to some embodiments of the present invention, the temperature of the etching and polishing is 25°C to 100°C.
[0071] Too low a temperature will reduce the rate of chemical reactions in the etching solution, resulting in a slow etching process and prolonged polishing time. The reactivity of the etching solution deteriorates at low temperatures, which may result in insufficient reaction between NH4OH and H2O2 in the etching solution, affecting the uniformity and quality of etching and making the reactivity difficult to control. High temperatures may cause the chemical components in the etching solution to decompose or become unstable, causing the etching solution to lose its original activity and effect. High temperatures may also cause surface denaturation or thermal damage to the lithium niobate material, deteriorating the surface quality of the optical waveguide and even causing deformation or cracks in the material.
[0072] Therefore, in order to ensure the effect and stability of the etching and polishing process, as well as the controllability and safety of the process, the etching and polishing temperature should be controlled within the range of 25°C to 100°C. Within this range, the etching rate, reaction uniformity and material stability can be balanced, thereby ensuring the quality and performance of the optical waveguide device preparation.
[0073] According to some embodiments of the present invention, the temperature of the etching and polishing is 50°C to 95°C.
[0074] According to some embodiments of the present invention, the temperature of the etching and polishing is 60°C to 85°C.
[0075] According to some embodiments of the present invention, the etching and polishing time is 5 min to 30 min.
[0076] Time control during the etching and polishing process is very important for ensuring the etching depth and surface quality. Normally, the etching and polishing time is controlled within the range of 5 minutes to 30 minutes, which can effectively control the etching depth and ensure the smoothness of the surface. Too short a time may result in insufficient etching depth, and the impurities and unevenness on the surface cannot be completely removed, affecting the optical performance and quality of the end face. Insufficient etching time may also cause the end face surface to be uneven or residual unetched areas, affecting the final performance of the optical waveguide device. If the time is too long, it will lead to excessive etching of the lithium niobate material, which may deteriorate the surface quality of the end face and even cause damage or deformation of the surface. In addition, too long an etching time will increase the manufacturing cycle and cost, and reduce the efficiency and economy of the process.
[0077] Therefore, in order to ensure the effect and stability of the etching and polishing process, as well as the controllability and economy of the process, the etching and polishing time should be strictly controlled within the range of 5 minutes to 30 minutes. Within this time range, the etching depth and surface smoothness can be effectively controlled, thereby ensuring the quality and performance of the optical waveguide device preparation.
[0078] According to some embodiments of the present invention, the etching and polishing time is 2 min to 25 min.
[0079] According to some embodiments of the present invention, the polishing method further comprises the step of placing the thin film lithium niobate optical waveguide chip in deionized water to remove residual solution after etching and polishing.
[0080] The NH4OH and H2O2 solutions used in the etching and polishing process may leave a small amount of chemical residue on the surface of the optical waveguide. Placing the chip in deionized water can effectively remove these residues and ensure the cleanliness and purity of the optical waveguide surface. Deionized water has high purity and low ion content, and will not cause secondary contamination or corrosion to the surface of the optical waveguide. This can ensure that the end face of the optical waveguide after etching and polishing maintains good chemical stability and optical properties. Deionized water can effectively reduce the impact of the medium on the performance of the optical waveguide and improve the stability and reliability of the device. This is especially important for optical devices that require long-term stable operation. Incorporating the deionized water cleaning step into the polishing method can improve the entire process flow and ensure the quality and consistency of each step. This helps to improve manufacturing efficiency and reduce defective rates.
[0081] According to some embodiments of the present invention, the polishing method further comprises the step of drying the thin film lithium niobate optical waveguide chip with nitrogen after removing the residual solution.
[0082] Nitrogen drying can effectively remove residual moisture and prevent water spots from being left on the surface of the device. This is particularly important for the optical performance of the optical waveguide, because water spots may cause scattering or loss of light transmission, and can prevent the device from undergoing oxidation reactions in the air, keeping the surface clean and stable. Using nitrogen to dry can also effectively avoid leaving ionic pollutants on the surface, which may affect the electrical properties and long-term stability of the optical waveguide. It is easy to understand that nitrogen drying is a fast and effective step that can quickly dry the surface of the device, shorten the manufacturing cycle, and improve production efficiency. In addition, nitrogen is a harmless and environmentally friendly gas. Using nitrogen to dry avoids the use of organic solvents or other drying methods that may be harmful to the environment, which meets the requirements of green manufacturing. The surface of the optical waveguide chip after drying is clean and free of water spots, and provides a clean and stable foundation for subsequent subsequent processing steps, such as packaging and testing of optical waveguide devices.
[0083] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0084] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0085] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.
[0086] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.
[0087] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0088] Example
[0089] Polishing of thin film lithium niobate optical waveguide chips, reference Figures 1 to 3 shown.
[0090] Figure 1 Flow chart of the polishing process.
[0091] Figure 2 A top view of the polishing process.
[0092] Figure 3 A side view of the polishing process.
[0093] The specific steps are:
[0094] (1) Depositing a silicon dioxide protective layer on the surface of the thin-film lithium niobate optical waveguide chip by PECVD. The specific process parameters are a thickness of about 1 μm;
[0095] (2) coating photoresist; the specific process parameters are that the thickness is about 1 μm;
[0096] (3) Cutting and splitting from the back side of the optical waveguide chip;
[0097] (4) Degumming: The specific method is as follows: first, soak the chip in an acetone solution for more than 5 minutes, then transfer it to an isopropanol solution and soak it for more than 5 minutes, and finally soak it in deionized water for more than 5 minutes, and use a nitrogen gun to blow dry the aqueous solution on the chip surface.
[0098] (5) Etching and polishing. The optical waveguide chip is placed in an etching and polishing polishing solution for polishing. The volume percentage of NH4OH in the etching and polishing polishing solution is 40 vol%. The volume ratio of NH4OH, H2O2 and deionized water is 2:2:1. The etching and polishing temperature is 85°C and the time is 10 min.
[0099] After etching and polishing, the thin-film lithium niobate optical waveguide chip is placed in deionized water to remove residual solution. After the residual solution is removed, the thin-film lithium niobate optical waveguide chip is blown dry with nitrogen.
[0100] The micro-optical morphology of the waveguide end face was observed by scanning electron microscopy.
[0101] Figure 4 It is the micro-optical morphology of the waveguide end face before the optical waveguide chip is placed in the polishing liquid for etching and polishing. Figure 4 It can be seen that the end face of the waveguide is relatively rough, with bumpy surface.
[0102] Figure 5 It is the micro-optical morphology of the waveguide end face after the optical waveguide chip is placed in the polishing liquid for etching and polishing. Figure 5 It can be seen that the roughness of the waveguide end face has been improved and the surface tends to be smooth and flat.
[0103] Comparative Example 1
[0104] Compared with the embodiment, the difference is that the polishing liquid for etching and polishing only contains NH4OH and deionized water, and the volume percentage of NH4OH is 40 vol%.
[0105] Comparative Example 2
[0106] Compared with the embodiment, the difference is that the polishing liquid for etching and polishing only contains H2O2 and deionized water, and the volume percentage of H2O2 is 40 vol%.
[0107] The test results of comparative examples 1 and 2 were compared with the embodiment, and it was found that when NH4OH or H2O2 was missing, the roughness of the waveguide end face was large and the surface was not smooth. Only by using NH4OH and H2O2 solutions for etching and polishing at the same time can the controllability and stability of the end face quality in the preparation process of the optical waveguide device be achieved.
[0108] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A polishing method for a thin-film lithium niobate optical waveguide chip, characterized in that: The method comprises the steps of depositing a protective layer on the surface of a thin-film lithium niobate optical waveguide chip, coating photoresist, cutting, degumming and etching and polishing, wherein the etching and polishing polishing liquid contains NH4OH and H2O2.
2. The polishing method according to claim 1, characterized in that: The protective layer includes a silicon dioxide protective layer.
3. The polishing method according to claim 1, characterized in that: The cut passes through the waveguide.
4. The polishing method according to claim 1, characterized in that: The polishing liquid for etching and polishing is an aqueous solution of NH4OH and H2O2.
5. The polishing method according to any one of claims 1 to 4, characterized in that: In the polishing liquid, the volume percentage of NH4OH is 20 vol% to 50 vol%.
6. The polishing method according to any one of claims 1 to 4, characterized in that: In the polishing liquid, the volume percentage of H2O2 is 20 vol% to 50 vol%.
7. The polishing method according to any one of claims 1 to 4, characterized in that: In the polishing liquid, the volume ratio of NH4OH, H2O2 and water is 2:2:
1.
8. The polishing method according to any one of claims 1 to 4, characterized in that: The temperature of the etching and polishing is 25°C to 100°C.
9. The polishing method according to any one of claims 1 to 4, characterized in that: The polishing method further comprises the step of placing the thin film lithium niobate optical waveguide chip in deionized water to remove residual solution after etching and polishing.
10. The polishing method according to claim 9, characterized in that: The polishing method further comprises the step of drying the thin-film lithium niobate optical waveguide chip with nitrogen after removing the residual solution.