Judgment method of round billet continuous casting quick change process mixing area
By establishing a circular continuous casting geometric model and simulating the transmission process of solidified heat transfer components of steel seeds, the problem of difficulty in judging the length of the mixing area in the rapid continuous casting process is solved, and accurate prediction and resource optimization are achieved.
Patent Information
- Application Number
- CN202411198528.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, the continuous casting quick replacement process is too long, and the length of the mixing area cannot be accurately judged, resulting in waste of costs and waste of raw materials.
By establishing an axisymmetric circular blank continuous casting geometric model, constructing a calculation domain, simulating the transmission process of solidification heat transfer components of steel seeds, calculating the concentration changes of solute elements in the mixed area, and determining the range of the mixed area.
Accurately predict the length of the handover blank, improve production efficiency, reduce cost consumption, and optimize resource utilization.
Smart Images

Figure CN119067010A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for determining a mixed area in a round billet continuous casting quick-change process. Background Art
[0002] As an efficient and continuous casting process, continuous casting technology has become an indispensable part of modern steel production. In the steel production process, the alternating casting of different steel grades is a common operation. When it is necessary to change the steel grade during the continuous casting process, a quick-change connector is usually used as the ingot starter for the new steel grade. This quick-change operation inevitably produces a section of the ingot with mixed composition, which is usually called the handover ingot.
[0003] Since the transfer billet contains a mixture of the previous and next two steel grades, it often does not meet the composition requirements of the final product, so it needs to be downgraded or directly treated as scrap steel. This phenomenon not only affects production efficiency, but also increases the waste of raw materials and production costs. Therefore, accurately predicting the length of the transfer billet is of great significance for achieving rapid and continuous continuous casting production and optimizing resource utilization.
[0004] At present, most of the research on the quick-change process of continuous casting is concentrated on the tundish. The tundish is a container for temporary storage and mixing of molten steel. The flow field and mixing behavior inside it have a direct impact on the length of the transfer billet. However, the mixing of molten steel is not limited to the tundish, but also occurs in the downstream crystallizer. Therefore, it is not comprehensive enough to only study the mixing situation in the tundish. In-depth research on the mixing behavior in the crystallizer is also required. Otherwise, it is impossible to judge the length of the mixing area, making the length of the transfer billet too long during production, wasting raw materials and generating a large amount of waste. Therefore, it is very important to judge the range of the mixing area in the tundish and the crystallizer. Summary of the invention
[0005] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a method for determining the mixed area of a round billet continuous casting quick-change process, which solves the technical problem in the prior art that the quick-change process takes too long and the length of the mixed area cannot be accurately determined, resulting in excessive cost waste.
[0006] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0007] The present invention provides a method for determining a mixing area in a round billet continuous casting quick-change process, comprising:
[0008] S1. Based on the processing plant information, a geometric model of axisymmetric round billet continuous casting is established, and based on the geometric model, a calculation domain is constructed;
[0009] The calculation domain includes connectors, crystallizer, secondary cooling zone and air cooling zone;
[0010] S2. Assign the material properties of the two pre-processed steel grades to separate calculation domains, and mesh the two calculation domains;
[0011] Among them, the two steel grades are new steel grade and old steel grade. Firstly, the axisymmetric round billet continuous casting geometric model of the old steel grade is established;
[0012] S3. According to the pre-established axisymmetric round billet continuous casting geometric model of the old steel grade, the solidification heat transfer component transmission process of the old steel grade is simulated, and stable temperature field distribution data and element distribution data are obtained to analyze and obtain the round billet continuous casting component transmission analysis model of the new steel grade;
[0013] S4. Stop pouring and drawing of the old steel grade, add connectors, and adhere the connectors to the billet shell to form a new steel grade ingot guide device; pour the new steel grade through the new steel grade ingot guide device, and calculate the change in solute element concentration in the mixing area according to different billet drawing speeds during the production of the new steel grade, and finally determine the range of the mixing area according to the solute element concentration distribution.
[0014] In some embodiments, the aforementioned method for determining the mixed area of the round billet continuous casting quick-change process, wherein in S1, the axisymmetric round billet continuous casting geometric model is a two-dimensional model, and the two-dimensional model includes: water inlet immersion depth data, crystallizer data, secondary cooling zone one data, secondary cooling zone two data, secondary cooling zone three data, secondary cooling zone four data and air cooling zone data, and the positional relationship of each item is arranged in sequence along the billet drawing direction.
[0015] In some embodiments, the aforementioned method for determining the mixed area of the round billet continuous casting quick-change process, wherein in S3, the solidification heat transfer component transfer process of the old steel grade includes, through the pre-set flow field boundary conditions, heat transfer conditions and component transfer boundary conditions of the calculation domain, combined with the flow field control equations, heat transfer control equations and component transfer equations of the calculation domain of the axisymmetric round billet continuous casting system, to obtain the round billet continuous casting component transfer analysis model of the old steel grade.
[0016] In some embodiments, the aforementioned method for determining the mixed area of the round billet continuous casting quick change process, wherein the temperature field distribution data in S3 is obtained according to formula (1)(2)(3)(4),
[0017]
[0018]
[0019]
[0020] k eff =f l ·k l+f s ·k s (4)
[0021] Where ρ is the solid density, is the velocity vector, H is the enthalpy change of the billet, C ps To express the specific heat capacity of solid, H ref is the enthalpy change at the reference temperature, T ref is the reference temperature, f l is the liquid fraction, f s is the solid fraction, k eff To consider the effect of turbulence on the effective thermal conductivity; T l 、T s are the liquidus temperature and the solidus temperature, respectively, l , k s are the thermal conductivity of liquid phase and the thermal conductivity of solid phase respectively;
[0022] The flow field distribution of the new steel ingot ingot device in S4 is obtained according to formulas (5)(6)(7)(8):
[0023]
[0024]
[0025]
[0026]
[0027] Where ρ is the solid density, is the velocity vector, are the solid phase velocity and liquid phase velocity, respectively, and f s , f l are the solid phase fraction and liquid phase fraction of the ingot, respectively; p is the operating pressure, μ eff is the effective viscosity, β T , β C,i are the thermal expansion coefficient and the solute expansion coefficient respectively, T is the calculation temperature; C i is the nominal concentration of element i, ref is the reference value of the physical quantity, A m is the permeability coefficient, u is the mixing velocity, S u is the source phase, where the first term on the right side of formula (7) represents the effect of temperature gradient and concentration gradient on thermal buoyancy and solute buoyancy during solidification; the second term represents the effect of enthalpy porosity;
[0028] The change of element concentration in S4 can be reflected from the element distribution data. The solute element component transmission data during round billet continuous casting can be obtained according to formula (9)(10)(11)(12)(13)(14):
[0029]
[0030]
[0031] C i =f s C s,i +f l C l,i (11)
[0032]
[0033]
[0034]
[0035] Among them, D s,i , D l,i are the diffusion coefficients of the solute elements in the solid phase and the liquid phase, C l,i , C s,i are the concentrations of the elements in the liquid phase and solid phase, Sc t is the Schmidt number, is the mixing speed, C i is the substance concentration. If the solidification system maintains thermodynamic equilibrium, the solute redistribution during the solidification process can be described by equations (12) and (13); C l,i , C s,i are the concentrations of the elements in the liquid phase and solid phase, respectively. The superscript is the value at the solid-liquid interface. L is the maximum length of the liquid core. D is the thickness of the ingot. v max is the maximum drawing speed, K is the solidification coefficient, the solidification coefficient of the large round billet is 28-30, and the solidification coefficient of the small round billet is 30-32.
[0036] In some embodiments, the aforementioned method for determining the mixed area of the round billet continuous casting quick-change process, wherein in S4, it can be determined whether the billet shell thickness meets the actual production safety thickness range, and the billet drawing speed corresponding to this billet shell thickness is combined as the optimal billet drawing speed for continuous casting of new steel round billets.
[0037] In some embodiments, the aforementioned method for determining the mixed area of the round billet continuous casting quick-change process, wherein, in S2, the content of the grid division includes: the submerged water nozzle, the crystallizer, the secondary cooling zone 1, the secondary cooling zone 2, the secondary cooling zone 3, the secondary cooling zone 4 and the air cooling zone during the round billet continuous casting process, wherein the shape of the connecting parts in S4 is subjected to encrypted grid division.
[0038] In some embodiments, the aforementioned method for determining the mixed area of the round billet continuous casting quick-change process, wherein the material properties of the steel type in S2 include: density, specific heat capacity, viscosity, thermal conductivity, enthalpy change, solid-liquid phase line temperature and thermal expansion coefficient, solute element equilibrium distribution coefficient, liquidus slope, eutectic temperature, diffusion coefficient and solute element expansion coefficient of the steel type.
[0039] In some embodiments, the aforementioned method for determining the mixed area of the round billet continuous casting quick change process, wherein the flow field boundary position includes the immersed nozzle, the model wall and the model outlet, wherein the k-epsilon turbulence equation is used, and the input parameters are as shown in formula (15)(16)(17)(18). According to the mass conservation law, the outlet is set to outflow, and the pouring temperature is the liquidus plus superheat.
[0040]
[0041]
[0042]
[0043] T in =T L +ΔT (18)
[0044] Among them, u cast u is the billet drawing speed; in is the casting speed of the billet; d in is the pouring inlet radius; d s is the radius of the billet; T in is the casting temperature; K in Set parameters for the turbulent kinetic energy at the inlet; T L is the liquidus temperature;
[0045] The heat transfer boundary positions include the top of the crystallizer, the crystallizer boundary, the wall of the submerged nozzle, the boundary of the secondary cooling area, the boundary of the air cooling area and the bottom of the ingot model; the air cooling area uses a radiation coefficient of 0.8 for heat transfer, and the bottom of the ingot model uses the outflow boundary for calculation, and no separate heat exchange is set;
[0046] The component transport boundary conditions include inlet component settings and boundary component settings, in which the lever-rule rule is used to calculate the component transport behavior.
[0047] In some embodiments, the aforementioned method for determining the mixed area of the round billet continuous casting quick-change process, wherein, in S4, turbulent behavior exists during the solidification process of the new steel round billet continuous casting, and the RNG k-epsilon turbulence model is used for analysis.
[0048] Through the above technical scheme, the method for determining the mixed area of the round billet continuous casting quick-change process proposed in the present invention is based on CFD software and, according to the process parameters in actual production, establishes a component transmission analysis model for the axisymmetric round billet continuous casting quick-change process, simulates the changes in the mixed areas of different steel grades at different casting speeds, and finally calculates the range of the mixed area at different casting speeds, and determines the best casting speed for the new steel grade that meets the model size quick-change process in combination with the billet shell thickness. Different casting speeds will change the flow and mixing characteristics of the molten steel in the tundish and crystallizer, thereby affecting the length of the handover billet, and realizing rapid and continuous continuous casting production and reducing cost consumption. In addition, in the method proposed in the embodiment of the present invention, the calculation of the quick-change connector is incorporated into the model analysis and calculation process, and compared with the prior art, the quick-change connector is simplified to a closed type;
[0049] In order to better understand and predict the length of the transfer billet, this paper established a two-dimensional mathematical model of the round billet continuous casting quick change process. Through this model, the mixing behavior of different steel grades during the quick change process was simulated and analyzed, especially the transfer billet length of steel grades Q355NE and 42CrMo during the quick change process was studied in detail. The establishment of the model and the simulation results provide a theoretical basis and data support for accurately predicting the length of the mixing area;
[0050] More efficient and economical steel production can be achieved by precisely controlling the mixing behavior of molten steel in the tundish and crystallizer. Through a comprehensive analysis of the mixing behavior in the tundish and crystallizer, an effective method for optimizing the continuous casting quick-change process is proposed, aiming to reduce the length of the mixing zone and improve production efficiency and product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 It is a schematic diagram of the process of an embodiment;
[0052] Figure 2 It is a mesh shape diagram of the geometric model of the continuous casting of the round billet of the old steel grade and the connecting parts in the embodiment;
[0053] Figure 3 It is a flow field diagram in the crystallizer of the geometric model of continuous casting of round billets of old steel grades in the embodiment;
[0054] Figure 4 The temperature diagram, liquid fraction diagram and element composition transmission diagram of the old steel grade in the round billet continuous casting quick change process in the embodiment;
[0055] Figure 5 (a) is a comparison diagram of the numerical simulation value and the measured value of the temperature field of steel grade Q355NE in the embodiment; Figure 5 (b) is a comparison chart of the numerical simulation value and the measured value of the shell thickness of the steel grade Q355NE in the embodiment;
[0056] Figure 6(a) is the carbon concentration variation range at 1 / 2 radius of the mixing area in the embodiment; Figure 6 (b) is the range of carbon concentration variation at the center of the mixing area in the embodiment;
[0057] Figure 7 (a) is a comparison chart of the simulated value and the measured value of the carbon concentration at 1 / 2 radius of the mixing area in the embodiment; Figure 7 (b) is a comparison chart of the simulated value and the measured value of the carbon concentration at the center of the mixing area in the embodiment;
[0058] Figure 8 (a) is a simulation diagram of the change in liquid fraction after the old steel grade generates a shell; Figure 8 (b) is a simulation diagram of the change in liquid fraction when the quick-change connector is placed when pouring is stopped; Figure 8 (c) is a simulation diagram of the change in liquid fraction of a new ingot ingot device formed by the connector and the new steel grade; Figure 8 (d) is a simulation diagram of the change in liquid phase fraction of the connector after running the calculation for 10 seconds when a new steel grade is added during the quick-change process.
[0059] Fig. 9 Schematic diagram of calculation results of mixed area when the casting speed of the new steel grade in the embodiment is 0.010m / s (a), 0.012m / s (b), and 0.016m / s (c);
[0060] Fig.10 Schematic diagram of concentration variation at 1 / 2 radius of the mixing area when the casting speed of the new steel grade in the embodiment is 0.010m / s (a), 0.012m / s (b), and 0.016m / s (c);
[0061] Fig.11 Schematic diagram of the change in element concentration at the center of the mixing area when the casting speed of the new steel type in the embodiment is 0.010m / s (a), 0.012m / s (b), and 0.016m / s (c). DETAILED DESCRIPTION
[0062] In order to better understand the above technical solution, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a clearer and more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0063] The embodiment of the present invention proposes a calculation method for the quick-change process of round billet continuous casting. The method takes into account the chemical composition, temperature gradient and fluid dynamics characteristics of different steel grades, and combines the component transmission lever rule (lever-rule) to perform numerical simulation calculations to obtain the distribution law of carbon element in the quick-change process of round billet continuous casting. The influence of thermal buoyancy and solute buoyancy is adjusted by introducing corresponding correction factors to more accurately reflect the physical phenomena in actual production. In addition, the method also incorporates the quick-change process into the simulation calculation to improve the accuracy and practicality of the model.
[0064] Embodiment 1
[0065] like Figure 1 As shown, this embodiment provides a method for determining a mixed area in a round billet continuous casting quick change process. The method of this embodiment can be implemented on any computer device. The method of this embodiment includes: the present invention relates to a round billet continuous casting quick change process
[0066] The mixed area determination method comprises: S1, establishing a geometric model of axisymmetric round billet continuous casting based on processing plant information, and constructing a calculation domain based on the geometric model; wherein the contents of the calculation domain include connectors, a crystallizer, a secondary cooling zone and an air cooling zone; S2, assigning the material properties of two pre-processed steel grades to separate calculation domains, and meshing the two calculation domains; wherein the two steel grades are a new steel grade and an old steel grade, and firstly establishing an axisymmetric round billet continuous casting geometric model of the old steel grade; S3, according to the pre-established axis of the old steel grade The round billet continuous casting geometric model is called to simulate the solidification heat transfer component transmission process of the old steel grade, and obtain stable temperature field distribution data and element distribution data to analyze and obtain the round billet continuous casting component transmission analysis model of the new steel grade; S4, stop the pouring and billet drawing of the old steel grade, add connecting parts, and the connecting parts are adhered to the billet shell to form a new steel grade ingot guide device; the new steel grade is poured through the new steel grade ingot guide device, and according to the different billet drawing speeds during the production of the new steel grade, the solute element concentration change in the mixing area is calculated, and finally the range of the mixing area is determined according to the solute element concentration distribution.
[0067] Specifically, Figure 2 As shown, in S1, an axisymmetric round billet continuous casting geometric model can be established according to actual production conditions, and the geometric model can be a two-dimensional geometric model or a three-dimensional geometric model; when the geometric model is a two-dimensional geometric model, the two-dimensional model includes: water inlet immersion depth data, crystallizer data, secondary cooling zone one data, secondary cooling zone two data, secondary cooling zone three data, secondary cooling zone four data and air cooling zone data, and the positional relationship of each item is arranged in sequence along the billet drawing direction, wherein the billet drawing direction is the gravity direction.
[0068] Specifically, in S2, the material properties of the steel grade are obtained by obtaining the phase diagram based on the thermodynamic calculation software. At the same time, according to the content of the main chemical components in different steel grades, the melting point, electrical conductivity, viscosity, density, thermal conductivity and specific heat of the steel grade can be determined by searching the database; according to the different carbon content in different steel grades, the solute element equilibrium distribution coefficient, liquidus slope, eutectic temperature, diffusion coefficient and solute element expansion coefficient of the steel grade are calculated according to the phase diagram;
[0069] At the same time, the contents of the computational domain that are meshed may include: immersion nozzle, quick-change connector, crystallizer area, secondary cooling zone 1, secondary cooling zone 2, secondary cooling zone 3, secondary cooling zone 4 and air cooling zone, such as Figure 2 As shown, the shape of the connector in S4 is meshed with encrypted mesh, wherein the encrypted mesh refers to meshing the corresponding calculation domain with a smaller step size, and the non-encrypted mesh refers to meshing the corresponding area with a larger step size; specifically, the step size of the non-encrypted mesh can be 5 to 10 times the step size of the encrypted mesh, and the step size of the encrypted mesh can be set according to actual needs. For example, for a round billet continuous casting system with a diameter of 300 mm, the step size of the encrypted mesh can be 2 mm to 5 mm.
[0070] Specifically, Figure 3 and Figure 4 As shown, the temperature field distribution data and element distribution data in S3 are usually implemented based on CFD (computational fluid dynamics) software. CFD software usually refers to a commercial CFD program. It is based on fluid mechanics and computer science. It can start from the calculation method and use the fast calculation power of the computer to obtain the approximate solution of the fluid control equation. In this embodiment, the CFD software can be any one of FLUENT software, CFX software, FloEFD software, AUTODESK CFD software, and PHOENICS software. Based on CFD software, the solidification heat transfer component transmission method is adopted to set the flow field control equation, heat transfer control equation and component transmission equation of the calculation domain of the axisymmetric round billet continuous casting system, and set the flow field boundary conditions, heat transfer conditions and component boundary conditions of the calculation domain to obtain the round billet continuous casting component transmission analysis model. The heat transfer boundary conditions, flow field boundary conditions and component transmission boundary conditions are usually selected and set according to the actual production situation.
[0071] Embodiment 2
[0072] In order to better understand the first embodiment, this embodiment takes the quick-change process of continuous casting of different steel grades Q355NE (old steel grade) and 42CrMo (new steel grade) with Ф300mm round billets as an example, and describes it in detail based on FLUENT software and combined with specific steps.
[0073] S1. Based on the actual factory information, a two-dimensional round billet continuous casting geometric model is established, and based on the geometric model, a calculation domain including a connector, a crystallizer, a secondary cooling zone and an air cooling zone is constructed;
[0074] Specifically, Figures 2 to 4 As shown in the figure, the parameters of each data in the two-dimensional model are: nozzle immersion depth 100mm, nozzle inner / outer diameter size Ф40 / 20mm, crystallizer length 780mm, secondary cooling zone 1 length 500mm, secondary cooling zone 2 length 1600mm, secondary cooling zone 3 length 2500mm, secondary cooling zone 4 length 5000mm, air cooling zone length 15000mm, connector width 25mm, connector upper and lower dimensions Ф250 / 220mm, connector length 450mm. The two-dimensional geometric model established based on the above data is shown in the figure. Figure 2 (a) shows that the calculation domain consists of the crystallizer zone 1, the secondary cooling zone 2 including the secondary cooling zone 1 (Zone 1), the secondary cooling zone 2 (Zone 2), the secondary cooling zone 3 (Zone 3), the secondary cooling zone 4 (Zone 4) and the air cooling zone 3; ① is the water inlet, ② is the outlet; Figure 2 (b) is the actual reference diagram of the connector; Figure 2 (c) is the mesh of the crystallizer area, and ① is a schematic diagram of the simulated mesh shape of the connector.
[0075] S2. Assign the material properties of the two pre-processed steel grades to separate calculation domains and mesh the two calculation domains.
[0076] Specifically, by searching the database or conducting experimental measurements, the material properties of Q355NE and 42CrMo are determined as shown in Table 1 below.
[0077] Table 1 Material property parameters of steel grades (Q355NE) and (42CrMO)
[0078]
[0079] S3. According to the pre-established axisymmetric round billet continuous casting geometric model of the old steel grade, the solidification heat transfer component transfer process of the old steel grade is simulated, and stable temperature field distribution data and element distribution data are obtained to analyze and obtain the component transfer analysis model of the round billet continuous casting of the new steel grade; wherein, the solidification heat transfer component transfer process of the old steel grade includes, based on the built-in VOF model of the FLUENT software, through the pre-set flow field boundary conditions, heat transfer conditions and component transfer boundary conditions of the calculation domain, combined with the flow field control equations, heat transfer control equations and component transfer equations of the calculation domain of the axisymmetric round billet continuous casting system, to obtain the component transfer analysis model of the round billet continuous casting of the old steel grade.
[0080] In this embodiment, based on FLUENT software and combined with the secondary developed user-defined program, a component transmission model of the round billet continuous casting quick change process including flow field, temperature field and component transmission is established for the round billet continuous casting quick change process. Figures 5 to 11 shown.
[0081] Among them, based on the temperature distribution data of round billet continuous casting, according to formula (1)(2)(3)(4), the formula is:
[0082]
[0083]
[0084]
[0085] k eff =f l ·k l +f s ·k s (4)
[0086] Where ρ is the solid density, is the velocity vector, H is the enthalpy change of the billet, C ps To express the specific heat capacity of solid, H ref is the enthalpy change at the reference temperature, T ref is the reference temperature, f l is the liquid fraction, f s is the solid fraction, k eff To consider the effect of turbulence on the effective thermal conductivity; T l 、T s are the liquidus temperature and the solidus temperature, respectively, l , k s are the liquid phase thermal conductivity and the solid phase thermal conductivity respectively. The numerical simulation value and the measured value of the temperature field of the old steel grade Q355NE can be compared, such as Figure 5 (a)
[0087] According to formula (5), (6), (7), (8), the flow field distribution of round billet ingot is obtained as follows:
[0088]
[0089]
[0090]
[0091]
[0092] Where ρ is the solid density, is the velocity vector, are the solid phase velocity and liquid phase velocity, respectively, and f s , f l are the solid phase fraction and liquid phase fraction of the ingot, respectively; p is the operating pressure, μ eff is the effective viscosity, β T , β C,i are the thermal expansion coefficient and the solute expansion coefficient respectively, T is the calculation temperature; C i is the nominal concentration of element i, ref is the reference value of the physical quantity, A m is the permeability coefficient, u is the mixing velocity, S u is the source phase;
[0093] The first term on the right side of formula (7) represents the effect of temperature gradient and concentration gradient on thermal buoyancy and solute buoyancy during solidification; the second term represents the effect of enthalpy porosity; this time, Darcy's law is used to describe that the porosity of each volume element is equal to the liquid fraction. Therefore, the porosity is equal to 1 in the liquid region and equal to 0 in the solid region, while the momentum decreases in the mushy region as the porosity increases. Permeability coefficient A m Usually depends on the pore morphology. In this model, A m It is calculated according to Minakawa as shown in formula (8).
[0094] The RNG k-epsilon turbulence model is used to study the turbulent behavior during the solidification process of round billet continuous casting. The control equation of the model is given by formula (19)(20)(21)(22):
[0095]
[0096]
[0097]
[0098]
[0099] In the formula, S k , S ε are the source terms of k and epsilon equations respectively; the low Reynolds number model and empirical parameters proposed by Launder and Sharma are shown in Table 2;
[0100] Table 2 Coefficients and empirical constants of the low Reynolds number model of the turbulence equation
[0101]
[0102] According to formulas (9)(10)(11)(12)(13)(14), the solute element component transport behavior during round billet continuous casting is obtained:
[0103]
[0104]
[0105] C i =f s C s,i +f l C l,i (11)
[0106]
[0107]
[0108]
[0109] D s,i , D l,i are the diffusion coefficients of the solute elements in the solid phase and the liquid phase, Sc t is the Schmidt number, and its value is shown in Table 1; the third term on the right side of formula (9) represents the convection source term, and the mixing velocity and substance concentration are shown in formulas (11) and (12);
[0110] In this paper, the lever rule is used to calculate the solute component transport behavior. Assuming that the solidification system maintains thermodynamic equilibrium, which means that the solute diffuses infinitely in the solid phase and the liquid phase, the solute redistribution during the solidification process can be described by equations (12) and (13). l,i , C s,i are the concentrations of the elements in the liquid phase and solid phase, respectively, and the superscript is the value at the solid-liquid interface. Formula (14) is the solution formula for the liquid core depth, where L is the maximum length of the liquid core; D is the thickness of the ingot, v max is the maximum drawing speed, K is the solidification coefficient, the solidification coefficient of the large round billet is 28-30, and the solidification coefficient of the small round billet is 30-32.
[0111] The flow field boundary conditions include the immersed nozzle, the model wall and the model outlet. This paper adopts the k-epsilon turbulence equation, and the input parameters are shown in formulas (15)(16)(17)(18). According to the mass conservation, the outlet is set to outflow, and the pouring temperature is the liquidus plus superheat.
[0112]
[0113]
[0114]
[0115] T in =T L +ΔT (18)
[0116] Among them, ucast u is the billet drawing speed; in is the casting speed of the billet; d in is the pouring inlet radius; d s is the radius of the billet; T in is the casting temperature;
[0117] The heat transfer boundary conditions include the top of the crystallizer, the crystallizer boundary, the wall of the submerged nozzle, the boundary of the secondary cooling area, the boundary of the air cooling area, and the bottom of the ingot model. This paper simplifies the model calculation, ignores the heat dissipation of the nozzle and the top of the crystallizer, and uses heat flow to transfer heat in the crystallizer area. The air cooling area is calculated based on the heat transfer coefficient equivalent to the water supply. The air cooling area uses a radiation coefficient of 0.8 for heat transfer. The bottom of the ingot is calculated using the outflow boundary, and no separate heat exchange is set.
[0118] Crystallizer area:
[0119]
[0120]
[0121]
[0122] Second cooling area:
[0123] q s =h(T surf -T cooling ) (18)
[0124]
[0125] Air cooling area:
[0126] q air =4.6·10 -8 [(T s +273) 4 -(T0+273) 4 ] (20)
[0127] Where, T surf is the surface temperature of the casting billet; T cooling is the cooling water temperature; q m is the heat flow in the crystallizer; Z m is the height of the crystallizer; q air is the radiation heat transfer coefficient; T s is the solidus line of the casting; T0 is the ambient temperature; Q W is the water supply to the secondary cooling area.
[0128] Among them, the component transport boundary conditions include inlet component settings and boundary component settings. This paper adopts the VOF model, defines the steel grade as a mixture, inputs it through an immersed nozzle, ignores the internal diffusion between elements, and uses the lever-rule rule to calculate the component transport behavior. At the same time, the effects of thermal buoyancy and solute buoyancy are considered, and the wall component diffusion flux is set to zero.
[0129] After calculating the round billet continuous casting model of the new steel grade, stop the pouring and billet drawing of the old steel grade, add the quick-change connector, wait until the connector is bonded to the formed billet shell to form a new ingot guide device, and then restart the pouring and billet drawing. The comparison between the numerical simulation value and the measured value of the billet shell thickness of the old steel grade Q355NE is shown in the figure below. Figure 5 As shown in (b), the pouring stop time is related to the model size and the material properties of the connecting parts. The formula used for pouring the new steel grade is shown in (9)(10)(11)(12)(13). The change of the mixed area under different casting speeds is calculated. According to the different casting speeds of the new steel grade, the change of element concentration in the mixed area is calculated. The range of the mixed area is determined according to the element concentration distribution. The specific range of carbon concentration change at 1 / 2 radius of the mixed area is as follows: Figure 6 As shown in (a), the comparison between the simulated value and the measured value of carbon concentration is Figure 7 As shown in (a), the carbon concentration range at 1 / 2 radius of the mixing area is as follows Figure 6 As shown in (b), the comparison between the simulated value and the measured value of carbon concentration at the center is shown in Figure 7 (b)
[0130] At the same time, considering whether the billet shell thickness meets the actual production safety thickness range, the continuous casting billet drawing speed is determined as the optimal billet drawing speed.
[0131] The method of the present invention is essentially based on the different carbon element concentrations, equilibrium distribution coefficients, and liquidus slopes of different steel grades, based on the pre-established round billet continuous casting component transmission analysis model, adding a quick-change connector to facilitate the formation of a new ingot starter. The changes in the mixed area of the new steel grade and the old steel grade under different casting speeds are calculated. Among them, the formation time of the ingot starter is related to the physical properties of the connector.
[0132] comprehensive Figure 7 , Fig.10 , Fig.11 As shown in Table 3, the optimal casting speed (0.014 m / s) of the Ø300 mm round billet continuous casting quick change process determined by this method meets the optimal production conditions for the measured mixed area and billet shell thickness. Fig. 9 It can be seen that the mixing area range of carbon elements under different casting speeds.
[0133] Table 3
[0134]
[0135] It will be appreciated by those skilled in the art that embodiments of the present invention may be provided as methods, systems or computer program products. Therefore, the present invention may take the form of a complete hardware embodiment, a complete software embodiment, or an embodiment combining software and hardware. Furthermore, the present invention may take the form of a computer program product implemented on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0136] The present invention is described with reference to the flowcharts and / or block diagrams of the methods, devices (systems) and computer program products according to the embodiments of the present invention. It should be understood that each process and / or box in the flowchart and / or block diagram, as well as the combination of the processes and / or boxes in the flowchart and / or block diagram, can be implemented by computer program instructions.
[0137] It should be noted that in the claims, any reference numerals placed between brackets shall not be construed as limiting the claims. The word "comprising" does not exclude the presence of components or steps not listed in the claims. The word "a" or "an" preceding a component does not exclude the presence of a plurality of such components. The invention may be implemented by means of hardware comprising several different components and by means of a suitably programmed computer. In the claims enumerating several means, several of these means may be embodied by the same hardware. The use of the words first, second, third, etc., is for convenience of expression only and does not indicate any order. These words may be understood as part of the component name.
[0138] In addition, it should be noted that, in the description of this specification, the description of the terms "one embodiment", "some embodiments", "embodiment", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0139] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments after knowing the basic creative concept. Therefore, the claims should be interpreted as including the preferred embodiments and all changes and modifications falling within the scope of the present invention.
[0140] Obviously, those skilled in the art can make various modifications and variations to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention should also include these modifications and variations.
Claims
1. A method for determining the mixed area of a round billet continuous casting quick change process, characterized in that: The steps include: S1. Based on the processing plant information, a geometric model of axisymmetric round billet continuous casting is established, and based on the geometric model, a calculation domain is constructed; The calculation domain includes connectors, crystallizer, secondary cooling zone and air cooling zone; S2. Assign the material properties of the two pre-processed steel grades to separate calculation domains, and mesh the two calculation domains; Among them, the two steel grades are new steel grade and old steel grade. Firstly, the axisymmetric round billet continuous casting geometric model of the old steel grade is established; S3. According to the pre-established axisymmetric round billet continuous casting geometric model of the old steel grade, the solidification heat transfer component transmission process of the old steel grade is simulated, and stable temperature field distribution data and element distribution data are obtained to analyze and obtain the round billet continuous casting component transmission analysis model of the new steel grade; S4. Stop pouring and drawing of the old steel grade, add connectors, and adhere the connectors to the billet shell to form a new steel grade ingot guide device; pour the new steel grade through the new steel grade ingot guide device, and calculate the change in solute element concentration in the mixing area according to different billet drawing speeds during the production of the new steel grade, and finally determine the range of the mixing area according to the solute element concentration distribution.
2. The method for determining the mixed area of the round billet continuous casting quick change process according to claim 1, characterized in that: In S1, the axisymmetric round billet continuous casting geometric model is a two-dimensional model, which includes: water inlet immersion depth data, crystallizer data, secondary cooling zone one data, secondary cooling zone two data, secondary cooling zone three data, secondary cooling zone four data and air cooling zone data, and the positional relationship of each item is arranged in sequence along the billet drawing direction.
3. The method for determining the mixed area of the round billet continuous casting quick change process according to claim 1, characterized in that: In S3, the solidification heat transfer component transfer process of the old steel grade includes obtaining the round billet continuous casting component transfer analysis model of the old steel grade through the pre-set flow field boundary conditions, heat transfer conditions and component transfer boundary conditions of the calculation domain, combined with the flow field control equations, heat transfer control equations and component transfer equations of the calculation domain of the axisymmetric round billet continuous casting system.
4. The method for determining the mixed area of the round billet continuous casting quick change process according to claim 1, characterized in that: The temperature field distribution data in S3 is obtained according to formula (1)(2)(3)(4): k eff =f l ·k l +f s ·k s (4) Where ρ is the solid density, is the velocity vector, H is the enthalpy change of the casting billet, C ps To express the specific heat capacity of solid, H ref is the enthalpy change at the reference temperature, T ref is the reference temperature, f l is the liquid fraction, f s is the solid fraction, k eff To consider the effect of turbulence on the effective thermal conductivity; T l 、T s are the liquidus temperature and the solidus temperature, respectively, l , k s are the thermal conductivity of liquid phase and the thermal conductivity of solid phase respectively; The flow field distribution of the new steel ingot ingot device in S4 is obtained according to formulas (5)(6)(7)(8): Where ρ is the solid density, is the velocity vector, are the solid phase velocity and liquid phase velocity, respectively, and f s , f l are the solid phase fraction and liquid phase fraction of the ingot, respectively; p is the operating pressure, μ eff is the effective viscosity, β T , β C,i are the thermal expansion coefficient and the solute expansion coefficient respectively, T is the calculation temperature; C i is the nominal concentration of element i, ref is the reference value of the physical quantity, A m is the permeability coefficient, u is the mixing velocity, S u is the source phase, where the first term on the right side of formula (7) represents the effect of temperature gradient and concentration gradient on thermal buoyancy and solute buoyancy during solidification; the second term represents the effect of enthalpy porosity; The change of element concentration in S4 can be reflected from the element distribution data. The solute element component transmission data during round billet continuous casting can be obtained according to formula (9)(10)(11)(12)(13)(14): C i =f s C s,i +f l C l,i (11) Among them, D s,i , D l,i are the diffusion coefficients of the solute elements in the solid phase and the liquid phase, C l,i , C s,i are the concentrations of the elements in the liquid phase and solid phase, Sc t is the Schmidt number, is the mixing speed, C i is the substance concentration. If the solidification system maintains thermodynamic equilibrium, the solute redistribution during the solidification process can be described by equations (12) and (13); C l,i , C s,i are the concentrations of the elements in the liquid phase and solid phase, respectively. The superscript is the value at the solid-liquid interface. L is the maximum length of the liquid core. D is the thickness of the ingot. v max is the maximum drawing speed, K is the solidification coefficient, the solidification coefficient of the large round billet is 28-30, and the solidification coefficient of the small round billet is 30-32.
5. The method for determining the mixed area of the round billet continuous casting quick change process according to claim 1, characterized in that: In S4, it can be determined whether the billet shell thickness meets the actual production safety thickness range, and the billet drawing speed corresponding to the billet shell thickness is combined as the optimal billet drawing speed during continuous casting of round billets of new steel grades.
6. The method for determining the mixed area of the round billet continuous casting quick change process according to claim 1, characterized in that: In S2, the mesh division content includes: the submerged nozzle, the crystallizer, the secondary cooling zone 1, the secondary cooling zone 2, the secondary cooling zone 3, the secondary cooling zone 4 and the air cooling zone during the round billet continuous casting process, wherein the shape of the connecting part in S4 is meshed encrypted.
7. The method for determining the mixed area of the round billet continuous casting quick change process according to claim 1, characterized in that: The material properties of the steel in S2 include: density, specific heat capacity, viscosity, thermal conductivity, enthalpy change, solid-liquid phase temperature and thermal expansion coefficient, solute element equilibrium distribution coefficient, liquidus slope, eutectic temperature, diffusion coefficient and solute element expansion coefficient of the steel.
8. The method for determining the mixed area of the round billet continuous casting quick change process according to claim 3, characterized in that: The flow field boundary positions include immersed nozzles, model walls and model outlets, wherein the k-epsilon turbulence equation is adopted, and the input parameters are as shown in formulas (15)(16)(17)(18). According to the law of conservation of mass, the outlet is set to outflow, and the pouring temperature is the liquidus plus superheat. T in =T L +ΔT (18) Among them, u cast u is the billet drawing speed; in is the casting speed of the billet; d in is the pouring inlet radius; d s is the radius of the billet; T in is the casting temperature; K in Set parameters for the turbulent kinetic energy at the inlet; T L is the liquidus temperature; The heat transfer boundary positions include the top of the crystallizer, the crystallizer boundary, the wall of the immersion nozzle, the boundary of the secondary cooling area, the boundary of the air cooling area and the bottom of the ingot model; wherein the air cooling area adopts a radiation coefficient of 0.8 for heat transfer, and the bottom of the ingot model adopts the outflow boundary for calculation, and no separate heat exchange is set; The component transport boundary conditions include inlet component settings and boundary component settings, wherein the lever-rule rule is used to calculate the component transport behavior.
9. The method for determining the mixed area of the round billet continuous casting quick change process according to claim 3, characterized in that: In S4, turbulent behavior exists during the solidification process of continuous casting of round billets of new steel grades, and the RNG k-epsilon turbulence model is used for analysis.
Citation Information
Cited By
Thermal analysis carbon control method for gray cast iron
CN121364757A