Cerium magnet with magnetic strengthening effect and different Fe content grain boundary phases and preparation method thereof
By controlling the Fe content and Ce distribution of the grain boundary phase in the cerium magnet, the problem of the coercive force of the cerium magnet decreases when Ce is replaced by Pr and Nd is solved, and the comprehensive magnetic performance and production stability of the cerium magnet are improved.
Patent Information
- Application Number
- CN202411257090.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-09
AI Technical Summary
When the proportion of Ce substitution Pr and Nd increases, the coercive force Hcj of the cerium magnet decreases, mainly due to the decrease in magnet performance caused by grain boundary phase composition and Ce element distribution, especially when Ce accounts for 0%-20% or 50% of the total rare earth content. It is significant in the range of %-80%.
By designing cerium magnets with grain boundary phases with different Fe contents, fine powders are prepared by quick-condensing and hydrogen breaking processes, and by airflow grinding and sintering heat treatment, the ratio and distribution of lean Fe phases and Fe-rich phases are controlled to ensure Ce Elements are distributed in the Fe-rich phase but not enriched in the main phase grains, thereby improving the magnetic isolation effect.
The comprehensive magnetic performance of cerium magnets is improved, and the mass production is more stable, avoiding a significant decrease in magnet performance when Ce increases, especially in different Ce content intervals to effectively maintain the coercive force Hcj.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnetic materials, in particular to a cerium magnet with magnetic strengthening effect and containing grain boundary phases with different Fe contents and a preparation method thereof. Background Art
[0002] With the popularization of automation and artificial intelligence technology, and the rapid development of magnetic material application fields such as new energy vehicles and wind power industries, the market demand for rare earth permanent magnet materials remains high. Due to the high prices of raw material metals Pr and Nd, related companies and technicians have begun to look for alternative elements to Pr and Nd. Ce has the most abundant reserves among rare earth elements, and its price is less than one-tenth of Pr and Nd. It has gradually attracted people's attention in recent years.
[0003] However, as the proportion of Ce replacing Pr and Nd increases, the coercivity Hcj of the magnet will gradually decrease. In actual production, this downward trend is particularly obvious when the Ce content in the magnet is in the range of 0%-20% or 50%-80% of the total rare earth content. This is mainly related to the grain boundary phase composition and Ce element distribution in the cerium magnet within this composition range.
[0004] When Ce accounts for 0%-20% of the total rare earth content, the grain boundary phase is mainly composed of the Fe-poor phase, which plays a role in magnetic isolation between the main phase grains and helps to improve the coercivity Hcj of the magnet. However, Ce is mainly distributed in the main phase grains to form the Ce2Fe14B phase, which has low intrinsic magnetic properties and is the main factor causing the decrease in the coercivity Hcj of the magnet.
[0005] When Ce accounts for 50%-80% of the total rare earth content, the grain boundary phase is mainly composed of Fe-rich phase, which is located at the intersection of triangular grain boundaries and cannot effectively play a magnetic isolation role. The removed Ce is distributed in the main phase grains and is mainly enriched in the grain boundaries to form a stable Fe-rich phase. At this time, the deterioration of the magnet microstructure is the main reason for the significant decline in performance.
[0006] In these two composition ranges, how to ensure the introduction of Ce elements and reduce the decrease of the coercive force Hcj of the magnet is a major difficulty. Summary of the invention
[0007] In view of the deficiencies in the prior art, the present invention provides a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents, and a preparation method thereof. The cerium magnet has better comprehensive magnetic properties.
[0008] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a cerium magnet with a magnetic strengthening effect and containing grain boundary phases with different Fe contents, characterized in that the nominal composition of the cerium magnet is (CexRE1-x)aFebalBbMc in mass percentage, wherein 0<x≤0.2 or 0.5≤x≤0.8, 29.5≤a≤33, 0.86≤b≤1.02, 0≤c≤5, bal is the remainder, RE is one or more of Pr, Nd, Gd, Td, Dy, Ho, Y, M is one or more of Co, Al, Cu, Ga, Nb, Ti, Zr, Mo, V, W The cerium magnet is composed of a main phase and a grain boundary phase, and the grain boundary phase contains an Fe-poor phase and an Fe-rich phase, wherein the composition of the Fe-poor phase is (CeyRE1-y)a1Fed1Mbal, 0≤y≤0.3, 70≤a1≤100, 0≤d1≤20, and the volume fraction of the Fe-poor phase in the grain boundary phase is A. The composition of the Fe-rich phase is (CezRE1-z)a2Fed2Bb2Mbal, 0≤z≤0.5, 10≤a2≤60, 40≤d2≤90, 0≤b2≤10, and the volume fraction of the Fe-rich phase in the grain boundary phase is B, and A and B satisfy the following conditions: 30%≤|AB|≤90%.
[0009] Preferably, the chemical formula of the Fe-rich phase includes but is not limited to CeFe2, CeFe2B2, Ce2Fe17, (CeRE)Fe2, (CeRE)6Fe13M1.
[0010] The present invention also provides another technical solution: a method for preparing a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents.
[0011] When x in the nominal composition of the cerium magnet satisfies 0<x≤0.2, the preparation method is as follows: 1) using a quick-setting process to refine at least one Ce-free quick-setting sheet containing a Fe-poor grain boundary phase and at least one Ce-rich quick-setting sheet containing a Fe-rich grain boundary phase, and then mixing the Ce-free quick-setting sheet and the Ce-rich quick-setting sheet in a certain proportion according to the final nominal composition of the cerium magnet; 2) Using hydrogen breaking process to break the mixed quick-setting sheets into hydrogen broken powder; 3) Use the jet milling process to break the hydrogen powder into fine powder with a particle size of 2-6μm; 4) After the fine powder is stirred and mixed, it is oriented and pressed to obtain a compact; 5) The green compact is subjected to a sintering heat treatment process to finally obtain a cerium magnet having a Fe-poor phase and a Fe-rich phase in the grain boundary phase.
[0012] Preferably, the nominal composition of the Ce-free quick-setting sheet containing the Fe-poor grain boundary phase is REaFebalBbMc in mass percentage, and the nominal composition of the Ce-rich quick-setting sheet containing the Fe-rich grain boundary phase is (CeuRE1-u)aFebalBbMc in mass percentage, 0.52≤u≤0.82.
[0013] When x in the nominal composition of the cerium magnet satisfies 0.5≤x≤0.8, the preparation method is as follows: 1) using a quick solidification process to refine at least one Ce-rich quick solidification sheet containing an Fe-rich grain boundary phase and at least one Ce-containing alloy sheet containing an Fe-poor grain boundary phase, and then mixing the Ce-rich quick solidification sheet and the Ce-containing alloy sheet in a certain proportion according to the final nominal composition of the cerium magnet; 2) Using hydrogen breaking process to break the mixed quick-setting sheets into hydrogen broken powder; 3) Use the jet milling process to break the hydrogen powder into fine powder with a particle size of 2-6μm; 4) After the fine powder is stirred and mixed, it is oriented and pressed to obtain a compact; 5) The green compact is subjected to a sintering heat treatment process to finally obtain a cerium magnet having a Fe-poor phase and a Fe-rich phase in the grain boundary phase.
[0014] Preferably, the nominal composition of the Ce-rich quick-setting sheet containing the Fe-rich grain boundary phase is (CevRE1-v)aFebalBbMc, 0.45≤v≤0.75, and the nominal composition of the Ce-containing alloy sheet containing the Fe-poor grain boundary phase is (CewRE1-w)a3Fed3Bb3Mbal, 0.1≤w≤0.8, 40≤a3≤100, 0≤d3≤60, 0≤b3≤0.96.
[0015] In the above two preparation methods, the sintering heat treatment process steps are as follows: 1) 950-1100℃ for 3-8h; 2) 850-950℃ for 0-5h; 3) 600-780℃ for 0-5h; 4) 350-550℃ for 0-5h.
[0016] Compared with the prior art, the present invention has the following advantages and effects: 1. When the Ce content x in the total rare earth content satisfies 0<x≤0.2, the magnet grain boundary phase is composed of a large number of Fe-poor phases and some Fe-rich phases. Ce is mainly distributed in the Fe-rich phase, which is not enriched in the main phase grains. At the same time, the Fe-poor phase plays a role in magnetic isolation between the main phase grains. In addition, only a small amount of Ce is needed to consume a large amount of Fe to form a stable Fe-rich phase, and the surplus rare earth enters the Fe-poor phase. The rare earth content in the Fe-poor phase increases, which can more effectively play a role in magnetic isolation between the main phase grains. Compared with the traditional single alloy process, the cerium magnets prepared by this method have better comprehensive magnetic properties and more stable mass production.
[0017] 2. When the Ce content in the total rare earth content x satisfies 0.5≤x≤0.8, the magnet grain boundary phase is composed of a part of Fe-poor phase and a large amount of Fe-rich phase. The existence of Fe-poor phase improves the microstructure of the magnet, ensuring that the magnet performance will not be significantly deteriorated even if there is a large amount of Fe-rich phase. DETAILED DESCRIPTION
[0018] The technical solutions in the embodiments of the present invention are clearly and completely described below. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0019] Example 1.
[0020] This embodiment provides a technical solution, a cerium magnet with a magnetic strengthening effect and containing grain boundary phases with different Fe contents and a preparation method thereof, which are specifically as follows: 1) First, the nominal composition of the cerium magnet is designed as (Ce0.11Pr0.09Nd0.8)29.9FebalB0.94Co0.3Al0.03Cu0.17Ga0.12Ti0.11Zr0.04, and then use the rapid setting process to refine the low Ce rapid setting sheet with the nominal composition of (Pr0.08Nd0.92)29.5FebalB0.95Co0.3Cu0.15Ga0.15Ti0.1Zr0.05 and the rich Ce rapid setting sheet with the nominal composition of (Ce0.53Pr0.12Nd0.35)31.51FebalB0.9Co0.3Al0.15Cu0.25Ti0.15, and the mixing ratio is 80:20; 2) Using hydrogen breaking process to break the mixed quick-setting sheets into hydrogen broken powder; 3) Use the jet milling process to break the hydrogen powder into fine powder with a particle size of 3-3.2μm; 4) After the fine powder is stirred and mixed, it is oriented and pressed to obtain a compact; 5) The pressed blanks were heat treated at 1075°C for 6.5 h, 900°C for 3 h, and 480°C for 5 h to obtain cerium magnets. The magnetic properties of the samples were tested using a permanent magnet material measuring instrument. The element distribution in the grain boundary phase of the magnet was analyzed using an electron probe to measure the proportion of Fe-poor phase and Fe-rich phase in the grain boundary.
[0021] Comparative example 1.
[0022] The cerium magnet is prepared by conventional single alloy process, as follows: The nominal composition of the product is (Ce0.11Pr0.09Nd0.8)29.9FebalB0.94Co0.3Al0.03Cu0.17Ga0.12Ti0.11Zr0.04) rapid solidification sheets; using hydrogen crushing process to crush the above rapid solidification sheets into hydrogen crushing powder; using air flow milling process to make the hydrogen crushing powder into fine powder with a particle size of 3-3.2μm; after stirring and mixing the fine powder, orient and press to obtain a pressed green sheet; the pressed green sheet is heat treated at 1075℃ for 6.5h, 900℃ for 3h, and 480℃ for 5h to obtain a cerium magnet.
[0023] The magnetic properties of cerium magnets and the proportions of Fe-poor and Fe-rich phases in the grain boundary phases are listed in Table 1.
[0024] Table 1 Magnetic properties of cerium magnets and the proportion of Fe-poor and Fe-rich phases in grain boundary phases sample Remanence Br (kGs) Coercivity Hcj (kOe) Squareness Hk / Hcj (%) The proportion of Fe-poor phase in grain boundary A (%) The proportion of Fe-rich phase in grain boundaries B (%) ∣AB∣(%) Example 1 14.35 12.11 98.2 92 8 84 Comparative Example 1 14.21 10.56 97.0 99 1 98 It can be seen from Table 1 that, compared with the conventional process, the comprehensive magnetic properties of the cerium magnet prepared in Example 1 of the present invention are more excellent.
[0025] Example 2.
[0026] In this embodiment, a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents and a preparation method thereof are specifically as follows: 1) First, the nominal composition of the cerium magnet is designed as (Ce0.5Pr0.12Nd0.38)32.14FebalB0.9Al0.1Cu0.2Ga0.1Ti0.1Zr0.4), and then the quick-setting process is used to refine the Ce-rich quick-setting sheet with a nominal composition of (Ce0.46Pr0.13Nd0.4)31.27FebalB0.92Al0.1Cu0.15Ti0.12Zr0.3 and the Ce-containing alloy sheet with a nominal composition of (Ce0.75Pr0.06Nd0.19)40FebalB0.9Al0.5Cu0.5Ga0.5Zr1, and the mixing ratio is 90:10; 2) Using hydrogen breaking process to break the mixed quick-setting sheets into hydrogen broken powder; 3) Use the jet milling process to crush the hydrogen powder into fine powder with a particle size of 3.2-3.5μm; 4) After the fine powder is stirred and mixed, it is oriented and pressed to obtain a compact; 5) The pressed blanks were heat treated at 1035°C for 5 h, 680°C for 5 h, and 480°C for 5 h to obtain cerium magnets, and the magnetic properties of the samples were tested using a permanent magnet material measuring instrument. The element distribution in the grain boundary phase of the magnet was analyzed using an electron probe to measure the proportion of Fe-poor phase and Fe-rich phase in the grain boundary.
[0027] Comparative example 2.
[0028] The cerium magnet is prepared by conventional single alloy process, as follows: The nominal composition of the product is (Ce0.47Pr0.13Nd0.4)32.21FebalB0.9Al0.1Cu0.2Ga0.1Ti0.1Zr0.4) quick-setting sheets; using hydrogen crushing process to crush the quick-setting sheets into hydrogen crushed powder; using air flow milling process to make the hydrogen crushed powder into fine powder with a particle size of 3.2-3.5μm; after stirring and mixing the fine powder, orient and press to obtain a pressed green sheet; the pressed green sheet is heat treated at 1035℃ for 5h, 680℃ for 5h, and 480℃ for 5h to obtain a cerium magnet.
[0029] The magnetic properties of cerium magnets and the proportions of Fe-poor and Fe-rich phases in the grain boundary phase are listed in Table 2.
[0030] Table 2 Magnetic properties of cerium magnets and the proportion of Fe-poor and Fe-rich phases in grain boundary phases sample Remanence Br (kGs) Coercivity Hcj (kOe) Squareness Hk / Hcj (%) The proportion of Fe-poor phase in grain boundary A (%) The proportion of Fe-rich phase in grain boundaries B (%) ∣AB∣(%) Example 2 12.11 12.53 97.7 14 86 72 Comparative Example 2 11.90 11.26 96.4 2 98 96 It can be seen from Table 2 that, compared with the conventional process, the cerium magnet prepared in Example 2 of the present invention has better comprehensive magnetic properties and a higher Ce content.
[0031] Example 3.
[0032] In this embodiment, a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents, the nominal composition of the cerium magnet is (CexRE1-x)aFebalBbMc by mass percentage, wherein x=0.2, a=33, b=1.02, c=5, bal is the remainder, RE is Dy, Ho and Y, and M is Ga, Nb and Ti; the cerium magnet is composed of a main phase and a grain boundary phase, and the grain boundary phase contains an Fe-poor phase and an Fe-rich phase, wherein, The composition of the Fe-poor phase is (CeyRE1-y)a1Fed1Mbal, y=0.3, a1=75, d1=20, and the volume fraction of the Fe-poor phase in the grain boundary phase is A. The composition of the Fe-rich phase is (CezRE1-z)a2Fed2Bb2Mbal, z=0.5, a2=15, d2=70, b2=10, and the volume fraction of the Fe-rich phase in the grain boundary phase is B. A and B satisfy the following conditions: |AB|=90%.
[0033] The preparation method is as follows: 1) using a quick-setting process to refine at least one Ce-free quick-setting sheet containing a Fe-poor grain boundary phase and at least one Ce-rich quick-setting sheet containing a Fe-rich grain boundary phase, and then mixing the Ce-free quick-setting sheet and the Ce-rich quick-setting sheet in a certain proportion according to the final nominal composition of the cerium magnet; 2) Using hydrogen breaking process to break the mixed quick-setting sheets into hydrogen broken powder; 3) Use the jet milling process to break the hydrogen powder into fine powder with a particle size of 2-6μm; 4) After the fine powder is stirred and mixed, it is oriented and pressed to obtain a compact; 5) The green compact is subjected to a sintering heat treatment process to finally obtain a cerium magnet having a Fe-poor phase and a Fe-rich phase in the grain boundary phase.
[0034] Among them, the nominal composition of the Ce-free quick-solidified sheet containing the Fe-poor grain boundary phase is REaFebalBbMc in mass percentage, and the nominal composition of the Ce-rich quick-solidified sheet containing the Fe-rich grain boundary phase is (CeuRE1-u)aFebalBbMc in mass percentage, where u=0.82.
[0035] The sintering heat treatment process steps are as follows: 1) 1100℃ for 5h; 2) 950℃ for 2h; 3) Keep at 700℃ for 1h; 4) Keep at 450℃ for 1h.
[0036] Example 4.
[0037] In this embodiment, a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents, the nominal composition of the cerium magnet is (CexRE1-x)aFebalBbMc by mass percentage, wherein x=0.8, a=31, b=0.92, c=2, bal is the remainder, RE is Nd and Gd, and M is Co, Al, and Zr; the cerium magnet is composed of a main phase and a grain boundary phase, and the grain boundary phase contains an Fe-poor phase and an Fe-rich phase, wherein the Fe-poor phase The composition of the Fe phase is (CeyRE1-y)a1Fed1Mbal, y=0.25, a1=85, d1=10, the volume fraction of the Fe-poor phase in the grain boundary phase is A, the composition of the Fe-rich phase is (CezRE1-z)a2Fed2Bb2Mbal, z=0.4, a2=30, d2=60, b2=1, the volume fraction of the Fe-rich phase in the grain boundary phase is B, A and B satisfy the following conditions: |AB|=30%.
[0038] The preparation method is as follows: 1) using a quick solidification process to refine at least one Ce-rich quick solidification sheet containing an Fe-rich grain boundary phase and at least one Ce-containing alloy sheet containing an Fe-poor grain boundary phase, and then mixing the Ce-rich quick solidification sheet and the Ce-containing alloy sheet in a certain proportion according to the final nominal composition of the cerium magnet; 2) Using hydrogen breaking process to break the mixed quick-setting sheets into hydrogen broken powder; 3) Use the jet milling process to break the hydrogen powder into fine powder with a particle size of 2-6μm; 4) After the fine powder is stirred and mixed, it is oriented and pressed to obtain a compact; 5) The green compact is subjected to a sintering heat treatment process to finally obtain a cerium magnet having a Fe-poor phase and a Fe-rich phase in the grain boundary phase.
[0039] Among them, the nominal composition of the Ce-rich quick-solidified sheet containing Fe-rich grain boundary phase is (CevRE1-v)aFebalBbMc, v=0.75, and the nominal composition of the Ce-containing alloy sheet containing Fe-poor grain boundary phase is (CewRE1-w)a3Fed3Bb3Mbal, w=0.8, a3=90, d3=5, b3=0.5.
[0040] The sintering heat treatment process steps are as follows: 1) 1000℃ for 7h; 2) 920℃ for 3h; 3) Keep at 750℃ for 5h; 4) Keep at 530℃ for 2h.
[0041] Although embodiments of the present invention have been shown and described, it will be apparent to those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and concepts of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents, characterized in that: The nominal composition of the cerium magnet is (CexRE1-x)aFebalBbMc by mass percentage, wherein 0<x≤0.2 or 0.5≤x≤0.8, 29.5≤a≤33, 0.86≤b≤1.02, 0≤c≤5, bal is the remainder, RE is one or more of Pr, Nd, Gd, Td, Dy, Ho, Y, and M is one or more of Co, Al, Cu, Ga, Nb, Ti, Zr, Mo, V, and W; the cerium magnet is composed of a main phase and a grain boundary phase, and the grain boundary phase contains F-poor e phase and Fe-rich phase, among which the composition of the Fe-poor phase is (CeyRE1-y)a1Fed1Mbal, 0≤y≤0.3, 70≤a1≤100, 0≤d1≤20, the volume fraction of the Fe-poor phase in the grain boundary phase is A, and the composition of the Fe-rich phase is (CezRE1-z)a2Fed2Bb2Mbal, 0≤z≤0.5, 10≤a2≤60, 40≤d2≤90, 0≤b2≤10, the volume fraction of the Fe-rich phase in the grain boundary phase is B, and A and B satisfy the following conditions: 30%≤|AB|≤90%.
2. The cerium magnet with different Fe content grain boundary phases having magnetic strengthening effect according to claim 1, characterized in that: The chemical formulas of the Fe-rich phase include CeFe2, CeFe2B2, Ce2Fe17, (CeRE)Fe2, (CeRE)6Fe13M1.
3. A method for preparing a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents as claimed in claim 1 or 2, characterized in that: When x in the nominal composition of the cerium magnet satisfies 0<x≤0.2, the preparation method is as follows: 1) using a quick-setting process to refine at least one Ce-free quick-setting sheet containing a Fe-poor grain boundary phase and at least one Ce-rich quick-setting sheet containing a Fe-rich grain boundary phase, and then mixing the Ce-free quick-setting sheet and the Ce-rich quick-setting sheet in a certain proportion according to the final nominal composition of the cerium magnet; 2) Use hydrogen breaking process to break the mixed quick-setting sheets into hydrogen breaking powder; 3) Use the jet milling process to break the hydrogen powder into fine powder with a particle size of 2-6μm; 4) After the fine powder is stirred and mixed, it is oriented and pressed to obtain a compact; 5) The green compact is subjected to a sintering heat treatment process to finally obtain a cerium magnet having a Fe-poor phase and a Fe-rich phase in the grain boundary phase; When x in the nominal composition of the cerium magnet satisfies 0.5≤x≤0.8, the preparation method is as follows: 1) using a quick solidification process to refine at least one Ce-rich quick solidification sheet containing an Fe-rich grain boundary phase and at least one Ce-containing alloy sheet containing an Fe-poor grain boundary phase, and then mixing the Ce-rich quick solidification sheet and the Ce-containing alloy sheet in a certain proportion according to the final nominal composition of the cerium magnet; 2) Use hydrogen breaking process to break the mixed quick-setting sheets into hydrogen breaking powder; 3) Use the jet milling process to break the hydrogen powder into fine powder with a particle size of 2-6μm; 4) After the fine powder is stirred and mixed, it is oriented and pressed to obtain a compact; 5) The green compact is subjected to a sintering heat treatment process to finally obtain a cerium magnet having a Fe-poor phase and a Fe-rich phase in the grain boundary phase.
4. The method for preparing a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents according to claim 3, characterized in that: When x in the nominal composition of the cerium magnet satisfies 0<x≤0.2, the nominal composition of the Ce-free quick-solidifying sheet containing the Fe-poor grain boundary phase is REaFebalBbMc in terms of mass percentage.
5. The method for preparing a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents according to claim 3, characterized in that: When x in the nominal composition of the cerium magnet satisfies 0<x≤0.2, the nominal composition of the Ce-rich quick-solidifying sheet containing the Fe-rich grain boundary phase is (CeuRE1-u)aFebalBbMc in mass percentage, 0.52≤u≤0.
82.
6. The method for preparing a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents according to claim 3, characterized in that: When x in the nominal composition of the cerium magnet satisfies 0.5≤x≤0.8, the nominal composition of the Ce-rich quick-solidifying sheet containing the Fe-rich grain boundary phase is (CevRE1-v)aFebalBbMc in mass percentage, 0.45≤v≤0.
75.
7. The method for preparing a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents according to claim 3, characterized in that: When x in the nominal composition of the cerium magnet satisfies 0.5≤x≤0.8, the nominal composition of the Ce-containing alloy sheet containing the Fe-poor grain boundary phase is (CewRE1-w)a3Fed3Bb3Mbal in mass percentage, 0.1≤w≤0.8, 40≤a3≤100, 0≤d3≤60, 0≤b3≤0.
96.
8. The method for preparing a cerium magnet having a magnetic strengthening effect and containing grain boundary phases with different Fe contents according to claim 3, characterized in that: The sintering heat treatment process steps are as follows: 1) 950-1100℃ insulation for 3-8h; 2) 850-950℃ insulation for 0-5h; 3) 600-780℃ insulation for 0-5h; 4) 350-550℃ insulation for 0-5h.
Citation Information
Patent Citations
Cerium-containing low-melting-point rare-earth permanent magnet liquid phase alloy and production method of permanent magnet comprising same
CN103280290A
Rare-earth permanent magnet and method of manufacturing the same
CN113496798A
RFeB BASED SINTERED MAGNET
JP2020013975A
Rare earth compound, method for producing the same, and use of the same
JP2023003525A
Soft magnetic alloy and magnetic device
US20190237229A1