Multi-layer composite barrier film as well as preparation method and application thereof

By forming two upper and lower aluminum oxide films on a flexible transparent substrate and introducing a multi-layer composite barrier film structure with an organic polysilazane layer, the problem of insufficient barrier performance in the prior art is solved, and high barrier and high light transmission are achieved Effect, suitable for packaging of flexible photovoltaic and electronic devices.

CN119069560AInactive Publication Date: 2024-12-03TIANJIN UNIV

Patent Information

Application Number
CN202411191834.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing flexible transparent ultra-high barrier films lack barrier performance when packaging flexible devices, making it difficult to meet the application needs of flexible photovoltaic and electronic devices.

Method used

A multi-layer composite barrier film structure is adopted, including a flexible transparent substrate and two upper and lower alumina films as barrier layers, and an organic polysilazane layer is introduced between the two inorganic oxides, and a plasma-enhanced atomic layer is deposited and sprayed/rotated by plasma-enhanced atomic layer. Preparation of coating composite process to form a high-quality barrier film.

Benefits of technology

The barrier properties and light transmittance of the film are significantly improved, the water vapor transmittance is ≤5×10-5g/(m2.day), and the light transmittance is ≥90%, extending the service life of flexible thin-film solar cells and OLED devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015317960000111
    Figure BDA0005015317960000111
  • Figure BDA0005015317960000121
    Figure BDA0005015317960000121
Patent Text Reader

Abstract

The invention relates to the technical field of films, and discloses a multi-layer composite barrier film and a preparation method and application thereof. The multilayer composite barrier film comprises a flexible transparent substrate, a barrier layer A arranged on one surface of the flexible transparent substrate, a polymer layer arranged on the surface of the barrier layer A, and a barrier layer B arranged on the surface of the polymer layer, the flexible transparent substrate is a flexible polymer film, and the thickness of the flexible transparent substrate is 50-150 microns; the barrier layer A and the barrier layer B are aluminum oxide films, and the thickness of the barrier layer A and the barrier layer B is 10-100 nm; the polymer layer is an organic polysilazane layer, and the thickness of the polymer layer is 100-1000 nm. According to the multilayer composite barrier film provided by the invention, the barrier performance of the film is greatly improved by arranging the upper and lower layers of inorganic oxides with specific thicknesses as the barrier layers; the polymer layer is introduced between the two inorganic matter layers, defect penetration caused by the too thick inorganic layer is avoided, the light transmittance performance is good, and the barrier property is further improved. The water vapor transmission rate of the multi-layer composite barrier film is smaller than or equal to 5 * 10 <-5 > g / (m2. Day), and the light transmittance is larger than or equal to 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of film technology, and in particular to a multi-layer composite barrier film and a preparation method and application thereof. Background Art

[0002] Flexible transparent high-barrier films have extremely low water vapor permeability and high light transmittance, and are widely used in flexible thin-film solar cells, organic electroluminescent devices (OLEDs), quantum dot displays, and other fields. Using flexible high-barrier films to effectively encapsulate devices can not only protect the products from external air and water erosion, extend their service life and maintain stable performance, but also do not affect the thinness, softness, and deformability of flexible device products, bringing breakthrough progress to the application of flexible products.

[0003] At present, the research and development of ultra-high barrier films mainly focuses on the design of film layer structure and preparation process. Studies have shown that inorganic barrier films prepared by atomic layer deposition (ALD) technology can achieve uniformity and consistency of the film layer, thereby obtaining excellent barrier properties. However, the barrier performance limit that can be achieved by a single-layer inorganic oxide barrier film is difficult to meet the packaging requirements of flexible devices. Therefore, researchers have developed a multi-layer barrier film to meet the needs of high barrier properties in specific application fields. Patent CN114507372A discloses a composite barrier film including a polymer base film, a first barrier layer, and a second barrier layer, wherein the first barrier layer and the second barrier layer include a fluorine-containing photosensitive resin, and the other layer includes a photosensitive resin, a silane coupling agent, and silicon-containing nanoparticles uniformly dispersed in the photosensitive resin and the silane coupling agent. The barrier film has a reduced cost and achieves a long-term and effective water and oxygen barrier effect, but due to its all-organic multi-layer structure, its barrier level is limited. Patent CN117301589A discloses a method for preparing a high barrier film for flexible display, wherein the barrier layer is formed by stacking one or more metal oxide thin films in any proportion, the light transmittance of the barrier film is greater than 88%, but the water vapor barrier performance is only 10 -3 g / (m 2 .day) level.

[0004] Therefore, there is an urgent need to develop a barrier film that has both ultra-high barrier properties and meets optical performance requirements to meet the application needs of flexible photovoltaic and electronic devices. Summary of the invention

[0005] The present application provides a multi-layer composite barrier film and a preparation method and application thereof, aiming to solve the problem of low barrier performance of existing flexible transparent ultra-high barrier films.

[0006] In order to achieve the above objectives, the present application adopts the following technical solutions.

[0007] In a first aspect of the present application, a multilayer composite barrier film is provided, comprising a flexible transparent substrate, a barrier layer A disposed on one side of the flexible transparent substrate, a polymer layer disposed on the surface of the barrier layer A, and a barrier layer B disposed on the surface of the polymer layer;

[0008] The flexible transparent substrate is a flexible polymer film with a thickness of 50 to 150 μm;

[0009] The barrier layer A and the barrier layer B are aluminum oxide films with a thickness of 10 to 100 nm;

[0010] The polymer layer is an organic polysilazane layer, and its thickness is 100-1000nm.

[0011] In some embodiments, the multi-layer composite barrier film further includes a transmittance-enhancing layer disposed on the surface of the barrier layer B, wherein the transmittance-enhancing layer is made of polysiloxane and has a thickness of 0.1 to 5 μm.

[0012] In some embodiments, the flexible transparent substrate includes any one of polyethylene terephthalate, polyethylene naphthalate, polycarbonate, or polyimide.

[0013] In some embodiments, the thickness of the flexible transparent substrate is 75 to 130 μm, and the light transmittance is > 80%;

[0014] The thickness of the barrier layer A and the deposition layer B is 30-60 nm;

[0015] The thickness of the polymer layer is 200-500 nm.

[0016] The second aspect of the present application provides a method for preparing the multi-layer composite barrier film, comprising:

[0017] S1, depositing an aluminum oxide film on the substrate surface as a barrier layer A by plasma enhanced atomic layer deposition;

[0018] S2, coating the surface of the barrier layer A with organic polysilazane by a spray coating / spin coating composite process, and obtaining a polymer layer after curing;

[0019] S3, performing hydrophilic treatment on the surface of the polymer layer, and depositing an aluminum oxide film on the surface by ion enhanced atomic layer deposition to obtain a barrier layer B.

[0020] In some embodiments, the preparation method further comprises:

[0021] S4, coating polysiloxane on the surface of the barrier layer B by a spray coating / spin coating composite process, and obtaining a transmittance-enhancing layer after curing.

[0022] In some embodiments, in S1 and S3, the deposition temperature of the plasma enhanced atomic layer deposition is 70-160°C.

[0023] In some embodiments, S2 specifically includes:

[0024] Spraying organic polysilazane on the surface of the substrate, then spin coating, and heating to cure after spin coating;

[0025] The rotation speed of the spin coating is 500-6000 rpm; the curing temperature is 50-100° C., and the curing time is 2-6 hours.

[0026] In some embodiments, the hydrophilic treatment comprises: performing plasma treatment on the polymer layer, wherein the power of the plasma is 200-300W.

[0027] The third aspect of the present application provides the use of the multilayer composite barrier film or the multilayer composite barrier film prepared by the above preparation method in a flexible thin-film solar cell or an organic electroluminescent device.

[0028] Compared with the prior art, the beneficial effects of this application are:

[0029] The multilayer composite barrier film of the present application has excellent light transmittance and high barrier performance by setting two layers of inorganic oxide of specific thickness as barrier layers. At the same time, a polymer layer is introduced between the two layers of inorganic materials to avoid the penetration of defects caused by the excessive thickness of the inorganic layer. The multilayer composite barrier film of the present application has good light transmittance and high barrier performance, and its water vapor transmission rate is ≤5×10 -5 g / (m 2 .day), light transmittance ≥ 90%.

[0030] The preparation method of the present application uses plasma enhanced atomic layer deposition technology to prepare inorganic oxide thin films, which can form high-quality films under low-temperature conditions that are more suitable for flexible substrates; before depositing the barrier layer, the surface of the organic layer is hydrophilically modified to provide a large number of active sites for the subsequent deposition of aluminum oxide, which is convenient for the growth of the film; the organic polymer film is prepared using a spray / spin coating composite process, which can achieve large-scale uniform coating, and the thickness can be controlled at the level of hundreds of nanometers. The multilayer composite barrier film prepared by the present application has high barrier properties and light transmittance, and is used in the encapsulation of flexible thin-film solar cells and organic electroluminescent devices (OLEDs), which can significantly improve their service life. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0032] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.

[0033] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0034] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0035] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0036] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0037] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be construed as specifically disclosing each intermediate value between the upper and lower limits of the scope. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.

[0038] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0039] In a first aspect, the present application provides a multilayer composite barrier film, comprising a flexible transparent substrate, a barrier layer A disposed on one side of the flexible transparent substrate, a polymer layer disposed on the surface of the barrier layer A, and a barrier layer B disposed on the surface of the polymer layer;

[0040] The flexible transparent substrate is a flexible polymer film with a thickness of 50-150 μm and a light transmittance of more than 80%, and more preferably a thickness of 75-130 μm. Specifically, the flexible transparent substrate can be any one of polyethylene terephthalate, polyethylene naphthalate, polycarbonate or polyimide.

[0041] The barrier layer A and the barrier layer B are aluminum oxide films with a thickness of 10 to 100 nm, more preferably 30 to 60 nm;

[0042] The polymer layer is an organic polysilazane layer, and its thickness is 100-1000 nm, and more preferably its thickness is 200-500 nm.

[0043] As a preferred solution, the multi-layer composite barrier film of the present application further comprises a transmittance-enhancing layer disposed on the surface of the barrier layer B to improve its light transmittance. The transmittance-enhancing layer is made of polysiloxane and has a thickness of 0.1 to 5 μm.

[0044] The multilayer composite barrier film of the present application has greatly improved the barrier performance of the film by setting two layers of inorganic oxides of specific thickness as barrier layers. At the same time, a polymer layer is introduced between the two layers of inorganic materials to avoid the penetration of defects caused by the excessive thickness of the inorganic layer, which can not only further improve the barrier performance, but also ensure that it has high light transmittance. The multilayer composite barrier film of the present application has good light transmittance and high barrier performance, and its water vapor transmission rate is ≤5×10 -5 g / (m 2 .day), light transmittance ≥ 90%.

[0045] In a second aspect, the present application provides a method for preparing the above-mentioned multi-layer composite barrier film, comprising:

[0046] S1, depositing an aluminum oxide film on the substrate surface as a barrier layer A by plasma enhanced atomic layer deposition;

[0047] Specifically, trimethylaluminum (TMA) is used as a precursor and oxygen plasma is used as an oxygen source, and a high-purity and high-uniformity aluminum oxide film is deposited on the surface of the substrate by plasma enhanced atomic layer deposition as the first barrier layer. The temperature of plasma enhanced atomic layer deposition is preferably 70 to 160° C., more preferably 90 to 140° C.; the plasma power is preferably 2500 to 3000 W.

[0048] S2, coating the surface of the barrier layer A with organic polysilazane by a spray coating / spin coating composite process, and obtaining a polymer layer after curing;

[0049] Specifically, first, the organic polysilazane is sprayed on the surface of the substrate, then spin-coated, and finally heated for curing. The spin-coating speed is 500-6000 rpm; the curing temperature is 50-100°C, and the curing time is 2-6 hours. Through the spray / spin coating composite process, a polymer layer with uniform thickness and texture is obtained, which greatly reduces the defects in the polymer layer and improves the light transmittance and barrier properties.

[0050] S3, performing hydrophilic treatment on the surface of the polymer layer, and depositing an aluminum oxide film on the surface by ion enhanced atomic layer deposition to obtain a barrier layer B.

[0051] Specifically, the product obtained in S2 is placed in a plasma treatment chamber, evacuated to a low vacuum state, and the surface of the polymer layer is plasma treated to introduce oxygen-containing groups such as hydroxyl groups on its surface, so that the surface has hydrophilic properties, providing more chemical reaction sites, which is conducive to the adsorption and reaction of the precursor material on its surface, thereby promoting the uniform deposition of the atomic layer and improving the film quality. The power of the plasma is preferably 200 to 300W.

[0052] On the hydrophilic polymer surface, a high-purity and high-uniformity aluminum oxide film is deposited by plasma enhanced atomic layer deposition as the second barrier layer. The temperature of the plasma enhanced atomic layer deposition is preferably 70 to 160°C, more preferably 90 to 140°C.

[0053] As a preferred solution, polysiloxane is deposited on the surface of the second barrier layer to improve its light transmission performance. Specifically, it includes:

[0054] S4, coating polysiloxane on the surface of the barrier layer B by a spray coating / spin coating composite process, and obtaining a transmittance-enhancing layer after curing.

[0055] Specifically, firstly, polysiloxane is sprayed on the surface of the barrier layer B, then spin-coated, and finally heated for curing. The spin-coating speed is 500-6000 rpm, the curing temperature is 50-100°C, and the curing time is 2-6 hours. Through the spray-coating / spin-coating composite process, a siloxane anti-transmittance layer with uniform thickness and texture is obtained, thereby improving the light transmission performance.

[0056] The multilayer composite barrier film of the present application, or the multilayer composite barrier film prepared by the present application in a flexible film, has good light transmittance and high barrier performance, and its water vapor transmission rate is ≤5×10 -5 g / (m 2 .day), light transmittance ≥ 90%, can be used in solar cells or organic electroluminescent devices OLED, improve their moisture and heat resistance and weather resistance, and can effectively increase the life of solar cells or OLED devices.

[0057] The present application is further described below by way of examples.

[0058] In the embodiment of the present application, the base material is a commercially available polymer film, and its specifications are as follows:

[0059] Polyethylene naphthalate (PEN) film (teonex Q65HA), thickness 100 μm, water vapor transmission rate 1.63 g / (m2.day), light transmittance 87.5%;

[0060] Polyethylene naphthalate (PEN) film (teonex Q65HA), thickness 125 μm, water vapor transmission rate 1.7 g / (m2·day), light transmittance 87.3%.

[0061] Polyethylene terephthalate film (PET) film (Toray U483, Japan), thickness 125 μm, water vapor transmission rate 5.06 g / (m2·day), light transmittance 89.5%.

[0062] OPSZ stands for organopolysilazane; PDMS stands for polydimethylsiloxane.

[0063] Example 1

[0064] This embodiment provides a method for preparing a multilayer composite barrier film, comprising:

[0065] S1, using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, a 40 nm thick aluminum oxide film is deposited on a 100 μm thick PEN substrate surface by plasma enhanced atomic layer deposition at 120°C as a barrier layer A;

[0066] S2, spraying the organic polysilazane on the surface of the barrier layer A, and then spin coating at a rotation speed of 5000 rpm to form an organic polysilazane layer with a thickness of 200 nm, and then curing at 80° C. for 3 hours to obtain a polymer layer;

[0067] S3, placing the product of S2 into a plasma treatment chamber, evacuating to a low vacuum state, setting the plasma treatment power to 250 W, and plasma treating the surface of the polymer layer for 8 minutes to perform hydrophilic modification; using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, a 40 nm thick aluminum oxide film is deposited on the surface of the polymer layer by plasma enhanced atomic layer deposition at 120°C as a barrier layer B.

[0068] Example 2

[0069] This embodiment provides a method for preparing a multilayer composite barrier film, comprising:

[0070] S1, using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, a 40 nm thick aluminum oxide film is deposited on a 125 μm thick PEN substrate by plasma enhanced atomic layer deposition at 120°C as a barrier layer A;

[0071] S2, spraying the organic polysilazane on the surface of the barrier layer A, and then spin coating at a rotation speed of 5000 rpm to form an organic polysilazane layer with a thickness of 500 nm, and then curing at 80° C. for 3 hours to obtain a polymer layer;

[0072] S3, placing the product of S2 into a plasma treatment chamber, evacuating to a low vacuum state, setting the plasma treatment power to 250 W, and plasma treating the surface of the polymer layer for 8 minutes to perform hydrophilic modification; using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, a 40 nm thick aluminum oxide film is deposited on the surface of the polymer layer by plasma enhanced atomic layer deposition at 120°C as a barrier layer B.

[0073] Example 3

[0074] This embodiment provides a method for preparing a multilayer composite barrier film having an anti-reflection layer, comprising:

[0075] S1, using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, a 40 nm thick aluminum oxide film is deposited on a 100 μm thick PEN substrate by plasma enhanced atomic layer deposition at 140°C as a barrier layer A;

[0076] S2, spraying the organic polysilazane on the surface of the barrier layer A, and then spin coating at a rotation speed of 5000 rpm to form an organic polysilazane layer with a thickness of 200 nm, and then curing at 80° C. for 3 hours to obtain a polymer layer;

[0077] S3, placing the product of S2 into a plasma treatment chamber, pumping to a low vacuum state, setting the power of the plasma treatment to 250 W, and plasma treating the surface of the polymer layer for 8 minutes to perform hydrophilic modification; using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, depositing an aluminum oxide film with a thickness of 40 nm on the surface of the polymer layer by plasma enhanced atomic layer deposition at 140°C as a barrier layer B;

[0078] S4, spraying polydimethylsiloxane on the surface of the barrier layer A, and then spin coating at a rotation speed of 5000 rpm to form a polydimethylsiloxane layer with a thickness of 500 nm, and then curing at 80° C. for 3 hours to form an anti-reflection layer.

[0079] Example 4

[0080] This embodiment provides a method for preparing a multilayer composite barrier film, comprising:

[0081] S1, using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, a 30 nm thick aluminum oxide film is deposited on the surface of a PET substrate by plasma enhanced atomic layer deposition at 120°C as a barrier layer A;

[0082] S2, spraying the organic polysilazane on the surface of the barrier layer A, and then spin coating at a rotation speed of 5000 rpm to form an organic polysilazane layer with a thickness of 200 nm, and then curing at 80° C. for 3 hours to obtain a polymer layer;

[0083] S3, placing the product of S2 into a plasma treatment chamber, evacuating to a low vacuum state, setting the plasma treatment power to 250 W, and plasma treating the surface of the polymer layer for 8 minutes to perform hydrophilic modification; using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, a 60 nm thick aluminum oxide film is deposited on the surface of the polymer layer by plasma enhanced atomic layer deposition at 120°C as a barrier layer B.

[0084] Example 3

[0085] This embodiment provides a method for preparing a multilayer composite barrier film having an anti-reflection layer, comprising:

[0086] S1, using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, a 50 nm thick aluminum oxide film is deposited on a 100 μm thick PEN substrate surface by plasma enhanced atomic layer deposition at 120°C as a barrier layer A;

[0087] S2, spraying the organic polysilazane on the surface of the barrier layer A, and then spin coating at a rotation speed of 5000 rpm to form an organic polysilazane layer with a thickness of 300 nm, and then curing at 80° C. for 3 hours to obtain a polymer layer;

[0088] S3, placing the product of S2 into a plasma treatment chamber, pumping to a low vacuum state, setting the power of the plasma treatment to 250 W, and plasma treating the surface of the polymer layer for 8 minutes to perform hydrophilic modification; using trimethylaluminum (TMA) as a precursor and oxygen plasma as an oxygen source, depositing an aluminum oxide film with a thickness of 40 nm on the surface of the polymer layer by plasma enhanced atomic layer deposition at 140°C as a barrier layer B;

[0089] S4, spraying polydimethylsiloxane on the surface of the barrier layer A, and then spin coating at a rotation speed of 5000 rpm to form a polydimethylsiloxane layer with a thickness of 1000 nm, and then curing at 80° C. for 3 hours to form an anti-reflection layer.

[0090] Comparative Example 1

[0091] The difference between Comparative Example 1 and Example 1 is that the organic polysilazane in step S2 is replaced by polyurethane acrylate to form a polyurethane acrylate layer with a thickness of 200 nm, and the rest is the same as Example 1.

[0092] Comparative Example 2

[0093] The difference between Comparative Example 2 and Example 1 is that the organic polysilazane in step S2 is replaced by polydimethylsiloxane to form a polydimethylsiloxane layer with a thickness of 200 nm, and the rest is the same as Example 1.

[0094] Comparative Example 3

[0095] The difference between Comparative Example 3 and Example 1 is that the temperature of plasma enhanced atomic layer deposition in steps S1 and S3 is 60° C., and the rest is the same as Example 1.

[0096] Comparative Example 4

[0097] The difference between Comparative Example 4 and Example 1 is that the thickness of barrier layer A and barrier layer B is 20 nm, and the rest is the same as Example 1.

[0098] Comparative Example 5

[0099] The difference between Comparative Example 5 and Example 1 is that the polymer surface is not hydrophilically modified in step S3, and the rest is the same as Example 1.

[0100] Comparative Example 6

[0101] The difference between Comparative Example 6 and Example 1 is that there is no step S2, and after the surface of the barrier layer A is hydrophilically modified, the barrier layer B is deposited on the surface thereof.

[0102] The multilayer composite barrier films prepared in Examples 1-5 and Comparative Examples 1-6 were characterized by testing water vapor transmission rate and light transmittance. The water vapor transmission rate was measured according to the GB / T 21529-2008 method, and the test instrument was the AQUATRAN model 3 moisture permeability tester of MOCON Company, USA. The test conditions were: 38°C, 90% RH, and the sample size was 10×10 cm; the light transmittance was measured according to the ASTM D1003-13 method. The test results are shown in Table 1.

[0103] Table 1 Test data of different multi-layer composite barrier films

[0104]

[0105]

[0106] As can be seen from Table 1, the water vapor transmission rate of the multilayer composite barrier film prepared in Examples 1-5 is ≤5×10 -5 g / (m 2 .day), light transmittance ≥ 90%, all of which have high barrier properties and high light transmittance. The water vapor transmission rate of the multilayer composite barrier film prepared in Comparative Examples 1-6 is 2.6×10 -2 -2.9×10 -4 g / (m 2 .day), both much higher than 5×10 -5 g / (m 2 .day).

[0107] The polymer layers of the multi-layer composite barrier films of Examples 1-5 have uniform surfaces and are basically defect-free after being coated with organic polysilazane; while the polymer layers of Comparative Examples 1 and 2 have poor surface uniformity and defects after being coated with polyurethane acrylate or PDMS, resulting in poor barrier properties of the final organic-inorganic composite barrier films.

[0108] The deposition temperature of the aluminum oxide film in Comparative Example 3 is low, the film quality is poor, and the barrier performance of the obtained multilayer composite barrier film is poor; the thickness of the aluminum oxide film in Comparative Example 4 is small, and the barrier performance of the obtained multilayer composite barrier film is also poor.

[0109] The polymer layer of Comparative Example 5 was not subjected to hydrophilic modification, and the barrier performance of the barrier film prepared therefrom was poor. Comparative Example 6 had no polymer layer, and the barrier performance and light transmittance of the barrier film prepared therefrom were both poor; in general, since there was no polymer layer to provide flexibility, the barrier film prepared in Comparative Example 6 had obvious cracks when stretched at a tensile strain of 5%.

[0110] Although the present application has been described in detail in general terms and in specific embodiments in this specification, it is obvious to those skilled in the art that some modifications or improvements may be made to the present application. Therefore, these modifications or improvements made without departing from the spirit of the present application are within the scope of protection claimed in the present application.

Claims

1. A multi-layer composite barrier film, characterized in that: It comprises a flexible transparent substrate, a barrier layer A disposed on one side of the flexible transparent substrate, a polymer layer disposed on the surface of the barrier layer A, and a barrier layer B disposed on the surface of the polymer layer; The flexible transparent substrate is a flexible polymer film with a thickness of 50 to 150 μm; The barrier layer A and the barrier layer B are aluminum oxide films with a thickness of 10 to 100 nm; The polymer layer is an organic polysilazane layer, and its thickness is 100-1000nm.

2. The multi-layer composite barrier film according to claim 1, characterized in that: It also includes a transmittance-enhancing layer disposed on the surface of the barrier layer B. The transmittance-enhancing layer is made of polysiloxane and has a thickness of 0.1 to 5 μm.

3. The multi-layer composite barrier film according to claim 1, characterized in that: The flexible transparent substrate includes any one of polyethylene terephthalate, polyethylene naphthalate, polycarbonate or polyimide.

4. The multi-layer composite barrier film according to claim 1, characterized in that: The thickness of the flexible transparent substrate is 75-130 μm, and the light transmittance is greater than 80%; The thickness of the barrier layer A and the deposition layer B is 30-60 nm; The thickness of the polymer layer is 200-500 nm.

5. The method for preparing a multilayer composite barrier film according to any one of claims 1 to 4, characterized in that: include: S1, depositing an aluminum oxide film on the substrate surface as a barrier layer A by plasma enhanced atomic layer deposition; S2, coating the surface of the barrier layer A with organic polysilazane by a spray coating / spin coating composite process, and obtaining a polymer layer after curing; S3, performing hydrophilic treatment on the surface of the polymer layer, and depositing an aluminum oxide film on the surface by ion enhanced atomic layer deposition to obtain a barrier layer B.

6. The preparation method according to claim 5, characterized in that: Also includes: S4, coating polysiloxane on the surface of the barrier layer B by a spray coating / spin coating composite process, and obtaining a transmittance-enhancing layer after curing.

7. The preparation method according to claim 5, characterized in that: In S1 and S3, the deposition temperature of the plasma enhanced atomic layer deposition is 70-160°C.

8. The preparation method according to claim 5, characterized in that: S2 specifically includes: Spraying organic polysilazane on the surface of the substrate, then spin coating, and heating to cure after spin coating; The rotation speed of the spin coating is 500-6000 rpm; the curing temperature is 50-100° C., and the curing time is 2-6 hours.

9. The preparation method according to claim 5, characterized in that: The hydrophilic treatment comprises: performing plasma treatment on the polymer layer, wherein the power of the plasma is 200-300W.

10. Use of the multilayer composite barrier film according to any one of claims 1 to 4 or the multilayer composite barrier film prepared by the preparation method according to any one of claims 5 to 9 in flexible thin-film solar cells or organic electroluminescent devices.

Citation Information

Patent Citations

  • Film packaging structure, preparation method and organic light emitting apparatus with same

    CN106299149A

  • Packaging method of flexible display and product

    CN110212108A

  • Organic metal halide perovskite solar cell composite packaging thin film and preparation method thereof

    CN110635044A

  • Flexible transparent ultra-low water vapor transmittance barrier film and preparation method thereof

    CN114515682A

  • Water-based anti-reflection coating liquid as well as preparation method and application thereof

    CN115678424A

Cited By

  • Flexible high-barrier film for electronic packaging and preparation method thereof

    CN120209726A