Preparation method of gallium oxide photoelectric detector with multilayer film structure
By adopting a multi-layer film structure with Ta layer and gallium oxide layer alternately in the gallium oxide detector, the problem of low carrier concentration is solved, and the photocurrent and responsiveness of the sun-blind ultraviolet detector is significantly improved, and better detection performance.
Patent Information
- Application Number
- CN202411024111.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-12-03
AI Technical Summary
The existing sun-blind ultraviolet detector materials such as AlGaN and ZnMgO have difficulties in preparation and performance, and the carrier concentration of gallium oxide is low, affecting the detection performance.
A multi-layer film structure with alternating Ta layer and gallium oxide layer is used, and prepared by magnetron sputtering method, which improves carrier concentration and optimizes film thickness and structure to enhance the detector performance.
It effectively improves the carrier concentration of the gallium oxide detector, enhances photocurrent and responsiveness, improves device performance, and is suitable for sun-blind ultraviolet light detection.
Smart Images

Figure CN119069581A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a solar-blind ultraviolet detector by utilizing a tantalum-gallium oxide multilayer film structure, and belongs to the technical field of semiconductor optoelectronics. Background Art
[0002] Solar Blind Ultraviolet (SBUV) detection technology is widely used and has attracted much attention from researchers. Sunlight in the SBUV (200-280 nm) band is almost completely absorbed when passing through the atmosphere, so detecting ultraviolet light in this band has the advantage of low background noise interference and is widely used in flame detection, missile tracking, space communications and ozone hole monitoring.
[0003] The materials currently used for solar-blind ultraviolet detectors are mainly AlGaN, ZnMgO, diamond, etc. However, there are many problems. For example, doping aluminum in gallium nitride will make it difficult to grow AlGaN epitaxial films, and as the Al content increases, the film quality is difficult to guarantee. In ZnMgO, the solubility between ZnO and MgO is not high, and phase separation will occur, so it is difficult to prepare wurtzite ZnMgO with a high Mg content. These reasons make these materials unsuitable for detecting solar-blind ultraviolet light.
[0004] The band gap of the ultra-wide bandgap semiconductor Ga2O3 is around 4.9 eV. It can directly detect solar-blind ultraviolet light without doping to adjust the bandgap width. It is a natural solar-blind ultraviolet detection material. Compared with the above materials, wide-bandgap semiconductor solar-blind ultraviolet detectors have the advantages of small size, low operating voltage, high temperature resistance, strong radiation resistance, etc., and have greater commercial value.
[0005] The preparation of Ga2O3 by magnetron sputtering has the advantages of fast speed, low cost, and uniform film quality, but gallium oxide has the problem of low photocurrent, that is, low carrier concentration. The most effective way to increase the carrier concentration is doping. Among them, the addition of Ta element can effectively increase the carrier concentration of gallium oxide. In order to better control the doping effect, the present invention proposes a multilayer film structure with alternating Ta layers and gallium oxide layers. Summary of the invention
[0006] Based on this background, the present invention provides a multi-layer film structure gallium oxide photodetector and a preparation method thereof
[0007] Explanation of terms
[0008] An interdigitated electrode is an electrode with a finger-like or comb-like appearance and a periodic pattern within the surface. This type of electrode is conducive to collecting carriers and increasing the device current.
[0009] The technical solution of the present invention is as follows:
[0010] A method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide comprises the following steps:
[0011] (1) polishing and cleaning the aluminum oxide substrate on one side or both sides to obtain a clean surface for depositing a gallium oxide-tantalum metal film;
[0012] (2) using a magnetron sputtering method, first sputtering a gallium oxide film on an aluminum oxide substrate, then sputtering a tantalum metal film on the basis of the sputtered gallium oxide film, and then sputtering the gallium oxide film again, and repeating this process 2-5 times to prepare a gallium oxide-tantalum metal film with a multilayer film structure, wherein the uppermost and lowermost layers of the gallium oxide-tantalum metal film are both gallium oxide films;
[0013] (3) cleaning the gallium oxide-tantalum metal film obtained in step (2), and then photolithographically defining the interdigitated electrode pattern using a photolithography process to prepare for the subsequent deposition of Ti-Au metal electrodes;
[0014] (4) Ti-Au metal electrodes were deposited by magnetron sputtering on the gallium oxide-tantalum metal film with the interdigital electrode pattern defined by photolithography to prepare the interdigital electrodes to obtain a gallium oxide solar-blind ultraviolet detector;
[0015] The photolithography-defined interdigital electrode pattern refers to preparing a designed interdigital electrode pattern on a prepared gallium oxide-tantalum metal film by using a photolithography process.
[0016] Furthermore, the aluminum oxide substrate is a (0001) oriented sapphire substrate; the thickness of each layer of the gallium oxide film is 50-125 nm, and the thickness of the tantalum metal layer is 0.1-5 nm to optimize the film quality;
[0017] The carrier concentration of the gallium oxide is 1×10 15 cm -3 ~1×10 19 cm -3 .
[0018] Furthermore, when depositing the gallium oxide film, the process parameters in the magnetron sputtering are as follows: the atmosphere in the preparation environment of the gallium oxide film is an argon-oxygen mixed gas, the oxygen flow rate is 1-4sccm, and the argon flow rate is 18-20sccm; the target material is a Ga2O3 ceramic target with a purity of 99.99% and a Ta metal target with a purity of 99.99%; the Ga2O3 sputtering power is 80-160W, and the Ta sputtering power is 100-150W; the substrate temperature is 25°C; the Ga2O3 sputtering time is 1000-3500s, and the Ta sputtering time is 3-150s;
[0019] Furthermore, the number of the interdigital electrode pairs is 5-20 pairs, and the finger width and finger distance are 5-20 μm;
[0020] Furthermore, the gallium oxide solar-blind ultraviolet detector is shaped like a finger or a comb, and has dimensions of 2-5 mm in length×1-3 mm in width×0.1-0.6 mm in height.
[0021] Furthermore, the gallium oxide multilayer film structure is Ga2O3-Ta- Ga2O3-Ta- Ga2O3-Ta- Ga2O3.
[0022] Furthermore, the gallium oxide film obtained in the cleaning step (2) refers to: using acetone for ultrasonic cleaning at a power of 40-60 W for 10-30 min, anhydrous ethanol for ultrasonic cleaning at a power of 40-60 W for 10-30 min, deionized water for ultrasonic cleaning at a power of 40-60 W for 10-30 min, centrifuging at 3000 r / min for 30 s, and drying in a constant temperature drying oven at 100° C. for 10-15 min.
[0023] Furthermore, in step (3), after the gallium oxide-tantalum film is spin-coated with photoresist, it is hardened in a constant temperature drying oven at 100° C. for 20-30 minutes, exposed with a mercury lamp for 20-30 seconds during photolithography, ultrasonically developed in a developer for 10-30 seconds, ultrasonically cleaned in deionized water for 1-2 minutes, and dried in a constant temperature drying oven at 100° C. for 10-20 minutes.
[0024] Furthermore, in step (4), when depositing Ti / Au on the gallium oxide-tantalum film, the process parameters in the magnetron sputtering are as follows: the atmosphere is argon gas, the argon gas flow rate is 18-20 sccm; the target material is a Ti metal target and an Au metal target; the sputtering power is 100-150 W; the substrate temperature is room temperature; and the sputtering time is 200-1000 s.
[0025] Furthermore, the tantalum metal layer can be replaced by other metal layers, including but not limited to elements such as Si, Sn, Ge, Nb, and W.
[0026] The innovation of the present invention is:
[0027] 1. The multi-layer film structure of the present invention can effectively improve the diffusion effect of the tantalum metal layer to the gallium oxide layer. The tantalum element has more valence electrons than the gallium element. After being doped, it can effectively increase the carrier concentration, thereby improving the photoelectric performance of the device.
[0028] 2. The radius of tantalum ion (0.64Å) is very close to that of gallium ion (0.62Å), which is conducive to the replacement of gallium by tantalum, thereby increasing the carrier concentration.
[0029] 3. The alternating structure of 2-5 layers can not only ensure the diffusion effect of the dopant, but also control the overall thickness to 200-500nm. The device performance of this film thickness is better.
[0030] The invention provides a method for preparing a multi-layer film structure gallium oxide photodetector, which has the advantages of being able to effectively improve the performance of the gallium oxide detector, increasing the number of carriers, and being able to increase the device photocurrent by 1-1000 times, thereby improving the device responsiveness.
[0031] The invention content described above further explains the purpose, technical scheme and other aspects of the present invention in detail. It should be noted that the above is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the principles of the present invention should be included in the protection scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the structure of a multi-layer film structure solar-blind ultraviolet detector;
[0033] Figure 2 It is a schematic diagram of the three-dimensional structure of a multi-layer film structure solar-blind ultraviolet detector;
[0034] [Description of Reference Numerals]
[0035] 1-interdigitated electrode, 2-Au electrode layer, 3-Ti electrode layer, 4-Ga2O3 thin film layer; 5-Ta thin film layer, 6-Al2O3 substrate layer. DETAILED DESCRIPTION
[0036] In order to make the technical solution of the present invention clearer, the present invention is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0037] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.
[0038] Example 1
[0039] A multi-layer film structure gallium oxide photodetector and a preparation method thereof, comprising the following steps:
[0040] (1) Polish and clean the aluminum oxide substrate on one side or both sides to obtain a clean surface for depositing the gallium oxide film. The specific cleaning method is: use acetone to ultrasonically clean for 10-30 minutes at a power of 40-60W, use anhydrous ethanol to ultrasonically clean for 10-30 minutes at a power of 40-60W, use deionized water to ultrasonically clean for 10-30 minutes at a power of 40-60W, use a centrifuge to rotate for 30 seconds at 3000r / min, and dry in a constant temperature drying oven at 100°C for 10-15 minutes, then take out and cool for use.
[0041] (2) Using magnetron sputtering, prepare the first layer of gallium oxide film on the aluminum oxide substrate with a thickness of 50-125nm. The specific parameters are: the background vacuum is better than 4×10 -5 Pa, the atmosphere in the preparation environment of gallium oxide film is argon-oxygen mixed gas, the oxygen flow rate is 1-4sccm, and the argon flow rate is 18-20sccm. The target material is 99.99% pure Ga2O3 ceramic target; Ga2O3 sputtering power is 80-160W; substrate temperature is 25℃. The sputtering time is 1000-3500s;
[0042] (3) epitaxially grow a tantalum metal layer on the first film with a thickness of 0.1-5 nm. The specific parameters are: the atmosphere in the preparation environment is argon gas, and the argon gas flow rate is 18-20 sccm. The target material is a 99.99% pure Ta metal target; the Ta sputtering power is 100-150 W; the substrate temperature is 25 ° C; the sputtering time is 3-150 s.
[0043] (4) Repeat step (2) on the tantalum metal layer. The stacking order of gallium oxide and tantalum film is as follows: Figure 1 As shown, there are 4 gallium oxide layers and 3 tantalum layers. However, this is not limited to this, and the number of layers can be changed according to specific requirements.
[0044] (5) Photolithography is performed on the top layer of gallium oxide to define the electrode pattern. After the gallium oxide film is spin-coated with photoresist, it is hardened in a constant temperature drying oven at 100°C for 20-30 minutes, and then the corresponding mask is selected, the exposure time is 20-30 seconds, ultrasonic development is performed in a developer for 10-30 seconds, ultrasonic cleaning is performed in deionized water for 1-2 minutes, and drying is performed in a constant temperature drying oven at 100°C for 10-20 minutes, and then taken out and cooled for use.
[0045] (6) Depositing metal Ti on the sample obtained in step (5) Using a magnetron sputtering instrument, the background vacuum is better than 4×10 - 5 Pa, argon flow rate is 18-20sccm, temperature is 25°C, target material is 99.99% purity Ti metal target, metal Ti is deposited on the sample surface with a thickness of 20-50nm, sputtering power is 100-150W, and sputtering time is 200-1000s.
[0046] (7) Depositing metal Au on the sample obtained in step (6) Using a magnetron sputtering instrument, the background vacuum is better than 4×10 - 5 Pa, argon flow rate is 18-20sccm, temperature is 25°C, target material is 99.99% purity Au metal target, metal Au is deposited on the sample surface with a thickness of 20-200nm, sputtering power is 100-150W, and sputtering time is 200-1000s.
[0047] (8) Debonding the sample obtained in step (7) and removing excess metal. Place the sample in a beaker and soak it in acetone solution for 1 hour; perform ultrasonic cleaning for 5-60 seconds until the excess metal is completely removed.
[0048] (9) The sample obtained in step (8) is cleaned by ultrasonication in deionized water for 30-60 seconds to remove excess acetone, and the sample is centrifuged at 3000 r / min for 30 seconds to remove excess water, and then moved to a 100°C constant temperature drying oven for drying for 10-15 minutes, and then removed and cooled for later use.
[0049] (10) Testing the sample obtained in step (9): observing the morphology under a microscope, and measuring the device performance using a semiconductor analyzer.
[0050] (11) Cut and package the sample with excellent performance in step (10) to obtain a multi-layer film gallium oxide solar-blind ultraviolet detector that can be used in an integrated manner.
Claims
1. A method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide, characterized in that: The steps include: (1) polishing and cleaning the aluminum oxide substrate on one side or both sides to obtain a clean surface for depositing a gallium oxide-tantalum metal film; (2) using a magnetron sputtering method, first sputtering a gallium oxide film on an aluminum oxide substrate, then sputtering a tantalum metal film on the basis of the sputtered gallium oxide film, and then sputtering the gallium oxide film again, and repeating this process 2-5 times to prepare a gallium oxide-tantalum metal film with a multilayer film structure, wherein the uppermost and lowermost layers of the gallium oxide-tantalum metal film are both gallium oxide films; (3) cleaning the gallium oxide-tantalum metal film obtained in step (2), and then photolithographically defining the interdigitated electrode pattern using a photolithography process to prepare for the subsequent deposition of Ti-Au metal electrodes; (4) Ti-Au metal electrodes are deposited by magnetron sputtering on a gallium oxide-tantalum metal film with a photolithographically defined interdigital electrode pattern to prepare interdigital electrodes to obtain a gallium oxide solar-blind ultraviolet detector; The photolithography-defined interdigital electrode pattern refers to preparing a designed interdigital electrode pattern on a prepared gallium oxide-tantalum metal film by using a photolithography process.
2. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: The aluminum oxide substrate is a sapphire substrate with a (0001) orientation; the thickness of each layer of the gallium oxide film is 50-125 nm, and the thickness of the tantalum metal layer is 0.1-5 nm to optimize the film quality; The carrier concentration of the gallium oxide is 1×10 15 cm -3 ~1×10 19 cm -3 .
3. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: When depositing gallium oxide film, the process parameters in magnetron sputtering are as follows: the atmosphere in the preparation environment of gallium oxide film is an argon-oxygen mixed gas, the oxygen flow rate is 1-4sccm, and the argon flow rate is 18-20sccm; the target material is a Ga2O3 ceramic target with a purity of 99.99% and a Ta metal target with a purity of 99.99%; the Ga2O3 sputtering power is 80-160W, and the Ta sputtering power is 100-150W; the substrate temperature is 25°C; the Ga2O3 sputtering time is 1000-3500s, and the Ta sputtering time is 3-150s.
4. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: The number of the interdigital electrode pairs is 5-20 pairs, and the finger width and finger distance are 5-20 μm.
5. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: The gallium oxide solar-blind ultraviolet detector has a finger-like or comb-like shape, and has a size of 2-5 mm in length×1-3 mm in width×0.1-0.6 mm in height.
6. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: The gallium oxide multilayer film structure is Ga2O3-Ta-Ga2O3-Ta- Ga2O3-Ta-Ga2O3.
7. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: The gallium oxide film obtained in the cleaning step (2) refers to: using acetone for ultrasonic cleaning at a power of 40-60W for 10-30min, anhydrous ethanol for ultrasonic cleaning at a power of 40-60W for 10-30min, deionized water for ultrasonic cleaning at a power of 40-60W for 10-30min, centrifuging at 3000r / min for 30s, and drying in a constant temperature drying oven at 100°C for 10-15min.
8. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: In step (3), the gallium oxide-tantalum film is spin-coated with photoresist, and then hardened in a constant temperature drying oven at 100° C. for 20-30 minutes, exposed with a mercury lamp for 20-30 seconds during photolithography, ultrasonically developed in a developer for 10-30 seconds, ultrasonically cleaned in deionized water for 1-2 minutes, and dried in a constant temperature drying oven at 100° C. for 10-20 minutes.
9. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: In step (4), when depositing Ti / Au on the gallium oxide-tantalum film, the process parameters in the magnetron sputtering are as follows: the atmosphere is argon gas, and the argon gas flow rate is 18-20 sccm; the target material is a Ti metal target and an Au metal target; the sputtering power is 100-150 W; the substrate temperature is room temperature, and the sputtering time is 200-1000 s.
10. The method for preparing a solar-blind ultraviolet detector using amorphous gallium oxide according to claim 1, characterized in that: The tantalum metal layer can be replaced by other metal layers, including but not limited to Si, Sn, Ge, Nb, and W elements.