Lithium nickel cobalt aluminate positive electrode material as well as preparation method and application thereof

By using a combination of polycrystalline strip-shaped large particles and single-crystal spherical small particles in the nickel-cobalt lithium aluminate positive electrode material, the surface rock salt structure and oxygen release of NCA materials under a wide voltage range are solved. The problem of improving circulation and thermal stability performance.

CN119069658APending Publication Date: 2024-12-03TIANJIN GUOAN MGL NEW MATERIALS TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310634847.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Nickel-cobalt lithium aluminate (NCA) cathode material has a NiO-like layer with a rock salt structure formed on the surface of primary particles under a wider charge and discharge voltage range, resulting in increased contact resistance and poor circulation performance, and releases high activity during charge and discharge. The oxygen causes the decomposition of PVDF binder and conductive carbon electrode, resulting in additional CO2, which cannot be effectively solved by the prior art.

Method used

By designing the combination of large particles and small particles, a combination of polycrystalline strip-shaped large particles and single-crystal spherical small particles is adopted, and a nickel-cobalt lithium aluminate coating is formed therein to enhance the bonding strength and grading effect between particles. To inhibit the formation of microcracks and lithosaline phases, anhydrous washing process and specific calcining conditions are used to prepare nickel-cobalt lithium aluminate positive electrode material.

Benefits of technology

The circulation performance and thermal stability of the nickel-cobalt lithium aluminate positive electrode material are significantly improved, the bonding strength and grading effect between particles are enhanced, the service life of the material is extended, and the occurrence of side reactions is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069658A_ABST
    Figure CN119069658A_ABST
Patent Text Reader

Abstract

The invention provides a nickel cobalt lithium aluminate positive electrode material and a preparation method and application thereof, the nickel cobalt lithium aluminate positive electrode material comprises a first particle and a second particle coated on the surface of the first particle, and a nickel cobalt lithium aluminate coating layer is arranged between the second particle and the first particle; the size of the first particles in the long axis direction is larger than that of the second particles in the long axis direction; each of the first particles and the second particles comprises nickel cobalt lithium aluminate; according to the lithium nickel cobalt aluminate positive electrode material, through structural design and matching of large and small particles, generation of microcracks is inhibited, meanwhile, generation of a NiO-like rock salt phase due to a side reaction between the surface of the material and an electrolyte is inhibited, and then the cycle performance and the thermal stability of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a nickel cobalt aluminum oxide lithium positive electrode material and a preparation method and application thereof. Background Art

[0002] As the core material of the four major materials of lithium-ion batteries, positive electrode materials play a vital role in the final performance of batteries. At present, the positive electrode materials of lithium-ion batteries used in industrial applications at home and abroad include lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and ternary (lithium nickel cobalt manganese oxide (NCM) and lithium nickel cobalt aluminum oxide (NCA)). Ternary materials are increasingly being paid attention to and recognized by the industry due to their dual advantages of comprehensive performance and cost, and gradually surpass lithium iron phosphate and lithium manganese oxide to become the mainstream technical route.

[0003] LiNi 1-x-y Co x Al y O2 (NCA) is a ternary positive electrode material with great commercial potential. It combines the advantages of LiNiO2 and LiCoO2. It not only has high reversible specific capacity and low material cost, but also enhances the structural stability and safety of the material after doping with aluminum (Al), thereby improving the material's cycle stability. Because of the above reasons, NCA material has become the focus of LiNiO2-based positive electrode material research, and it has achieved large-scale commercial application.

[0004] Although NCA positive electrode materials have certain advantages in terms of price and capacity, there are still some urgent problems that need to be solved. First, under a wider range of charge and discharge voltages, a NiO-like layer with a rock salt structure is formed on the surface of the primary particles of NCA, which increases the contact resistance between the particles and deteriorates the cycle performance. Second, NCA materials release oxygen during the charge and discharge process. The released oxygen is highly active and can cause the decomposition of PVDF binder and conductive carbon electrode carbon, thereby generating additional CO2 at lower temperatures than expected.

[0005] In the prior art, doping and coating are usually used to improve the defects of NCA materials. For example, CN108550802A discloses a Y / La-doped Co / B-coated nickel-cobalt-manganese ternary positive electrode material and a preparation method. A compound containing yttrium and lanthanum is added to a high-speed mixer together with a nickel-cobalt-manganese precursor and a lithium source for thorough mixing, and then calcined to obtain a doped material, thereby improving the stability of the material's crystal structure, thereby improving the material's cycle life and safety performance; CN112811403A provides a method for preparing a high-nickel ternary positive electrode material coated with Mg / Ti co-doped Li3PO4 in order to improve the electrochemical stability of high-nickel ternary positive electrode materials and improve battery rate performance and cycle performance; However, the above methods cannot solve the problem of the formation of a NiO-like layer with a rock salt structure on the surface of the primary particles of NCA.

[0006] Based on the above research, it is necessary to provide a nickel cobalt aluminum oxide positive electrode material, which can inhibit the generation of microcracks and the formation of a rock salt-like NiO layer, thereby effectively improving the cycle performance and thermal stability of the NCA material. Summary of the invention

[0007] The object of the present invention is to provide a nickel cobalt aluminum oxide positive electrode material and a preparation method and application thereof. The nickel cobalt aluminum oxide positive electrode material suppresses the generation of microcracks through structural design and the matching of large and small particles, and at the same time suppresses the side reaction between the surface of the material and the electrolyte to generate a NiO rock salt phase, thereby improving the cycle performance and thermal stability of the material.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a nickel cobalt aluminum oxide positive electrode material, wherein the nickel cobalt aluminum oxide positive electrode material comprises a first particle and a second particle coated on the surface of the first particle, and a nickel cobalt aluminum oxide coating layer is further included between the second particle and the first particle;

[0010] The size of the first particle in the long axis direction is greater than the size of the second particle in the long axis direction;

[0011] The first particles and the second particles both include lithium nickel cobalt aluminum oxide.

[0012] The size of the first particle in the long axis direction of the present invention is larger than the size of the second particle in the long axis direction, that is, the first particle in the present invention is a large particle, and the second particle is a small particle. The small particle is coated on the surface of the large particle, and a nickel cobalt aluminum oxide lithium coating layer is coated between the large and small particles. The presence of the coating layer improves the grading effect of the large and small particles, and also improves the bonding strength between the large and small particles, thereby further improving the cycle performance and thermal stability of the positive electrode material.

[0013] Preferably, the first particles are polycrystalline strip-shaped primary fiber particles, and the second particles are single-crystal spherical particles.

[0014] The first particles and the second particles of the present invention have different morphologies. Compared with the combination of large spherical particles and small spherical particles, the use of large polycrystalline strip-shaped primary fiber particles and single-crystal spherical small particles can further improve the grading effect.

[0015] Preferably, the size of the first particles in the long axis direction is larger than the primary particle size of the second particles.

[0016] Preferably, the size of the first particles in the minor axis direction is smaller than the primary particle size of the second particles.

[0017] Preferably, the first particles and the second particles are independently doped with doping elements, and the doping elements include any one of Zr, Sr or W or a combination of at least two of them, preferably a combination of Zr, Sr and W.

[0018] Preferably, the lithium nickel cobalt aluminum oxide coating layer is further doped with a doping element, and the doping element includes any one of Ti, Ce, W, La or Mg, or a combination of at least two of them.

[0019] In a second aspect, the present invention provides a method for preparing the lithium nickel cobalt aluminum oxide positive electrode material as described in the first aspect, the preparation method comprising the following steps:

[0020] (1) mixing and sintering the first particles, the cobalt source and the nickel source to obtain the first particles with the cobalt-nickel compound coated on the surface;

[0021] (2) Mixing and sintering the aluminum source and the second particles of the surface-coated lithium source with the first particles of the surface-coated cobalt-nickel compound in step (1) to obtain the nickel cobalt aluminum oxide positive electrode material.

[0022] The present invention, on the basis of grading large and small particles, coats a cobalt-nickel compound on the surface of a first particle, and then mixes and sinters with an aluminum source and a second particle coated with a lithium source on the surface, thereby in situ generating a nickel-cobalt-aluminum-oxide coating layer on the surfaces of the first particle and the second particle, thereby improving the bonding strength between the first particle and the second particle, thereby improving the stability of the material. Compared with directly preparing a nickel-cobalt-aluminum-oxide coating layer on the first particle, the present invention coats the first particle and the second particle separately and then sinters the first particle and the second particle together, thereby having a higher bonding strength between the particles and having better material performance.

[0023] In addition, the first particle of the present invention is first mixed with the cobalt source and the nickel source to prepare the first particle with the surface coated with the nickel-cobalt compound, and then mixed with the aluminum source and the second particle with the surface coated with the lithium source for sintering. Compared with first preparing the nickel-cobalt-aluminum compound on the surface of the first particle, the aluminum source is subsequently added in the present invention, which can react with LiPF6 to generate LiPO2F2, and LiPO2F2 is currently recognized as an electrolyte additive that is beneficial to battery performance, thereby improving the material performance. At the same time, the subsequent addition of the aluminum source can simultaneously inhibit the Ni on the surface of the first particle and the second particle. 3+ Reduction to Ni 2+ , lattice oxygen anion O 2- Oxidized into active oxygen anions O - , reduce surface residual alkali and improve the electrochemical properties of the material.

[0024] In the preparation method of the present invention, no water washing is performed, and a water-free washing process route is adopted.

[0025] Preferably, in step (1), the ratio of the size of the first particle in the short axis direction to the primary particle size of the second particle coated with the lithium source on the surface is 1:(6-10), for example, it can be 1:6, 1:7, 1:8, 1:9 or 1:10, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] In order to further enhance the matching effect of the first and second particles, the present invention further limits the ratio of the size of the first particle in the short axis direction to the primary particle size of the second particle coated with a lithium source on the surface, based on the specific morphology of the first particle and the second particle, thereby further enhancing the stability and electrochemical performance of the material.

[0027] Preferably, in step (1), the ratio of the size of the first particle in the long axis direction to the size in the short axis direction is (20-100):1, for example, it can be 20:1, 50:1 or 100:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] The thin strip-shaped primary fiber particles of the present invention partially dissipate the internal strain caused by the H2→H3 lattice distortion. A large number of inter-particle boundaries in the material serve as the priority positions for crack formation and propagation, releasing strain energy and ultimately improving the material's cycle performance and thermal stability.

[0029] Preferably, in step (1), the size of the first particles in the long axis direction is 5-10 μm, for example, 5 μm, 8 μm or 10 μm, and the size in the short axis direction is 0.06-0.3 μm, for example, 0.06 μm, 0.1 μm, 0.2 μm or 0.3 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the first particles in step (1) are prepared by the following method:

[0031] The first precursor and the lithium source are mixed and then calcined once to obtain the first particles.

[0032] Preferably, a doping source is also added during the mixing of the first precursor and the lithium source, and the doping source includes any one of a zirconium source, a strontium source or a tungsten source or a combination of at least two of them, preferably a combination of a zirconium source, a strontium source and a tungsten source.

[0033] Preferably, based on the mass of the first particle, the doping amount of the zirconium source is 0.08-0.20wt%, for example, it can be 0.08wt%, 0.1wt% or 0.20wt%, the doping amount of the strontium source is 0.08-0.20wt%, for example, it can be 0.08wt%, 0.1wt% or 0.20wt%, the doping amount of the tungsten source is 0.12-0.35wt%, for example, it can be 0.12wt%, 0.2wt%, 0.3wt% or 0.35wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the particle size of the first precursor is 10-17 μm, for example, 10 μm, 12 μm, 14 μm, 16 μm or 17 μm, and the BET is 1-4 μm. 2 / g, for example, 1m 2 / g, 2m 2 / g, 3m 2 / g or 4m 2 / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] Preferably, the molar ratio of lithium ions in the lithium source to total metal ions in the first precursor is (1.0-1.05):1, for example, 1.0:1, 1.03:1 or 1.0-1.05:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the primary calcination temperature is 650-800°C, such as 650°C, 700°C, 750°C or 800°C, the time is 10-30h, such as 10h, 20h or 30h, and the atmosphere is an oxygen atmosphere.

[0037] The present invention regulates the morphology of the first particle and the size in the major axis and minor axis directions through the synergistic effect among the zirconium source, the strontium source and the tungsten source, the selection of the precursor particle size and the control of the calcination conditions.

[0038] Preferably, the sintering temperature in step (1) is 550-650°C, for example, 550°C, 600°C or 650°C, the sintering time is 3-15h, for example, 3h, 5h, 10h or 15h, and the atmosphere is oxygen atmosphere.

[0039] Preferably, the cobalt source in step (1) includes any one of Co3O4, CoOOH, Co(OH)2 or CoCO3, or a combination of at least two thereof.

[0040] Preferably, the nickel source in step (1) comprises any one of NiOOH, Ni(OH)2, NiCO3 or NiO, or a combination of at least two of them.

[0041] Preferably, based on the mass of the first particles of the surface-coated cobalt-nickel compound in step (1), the amount of the cobalt source added in step (1) is 0.08-0.32wt%, for example, it can be 0.08wt%, 0.1wt%, 0.2wt% or 0.32wt%, and the amount of the nickel source added in step (1) is 0.08-0.32wt%, for example, it can be 0.08wt%, 0.1wt%, 0.2wt% or 0.32wt%.

[0042] Preferably, the primary particle size of the second particles coated with the lithium source in step (2) is 0.5-2.4 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2.0 μm or 2.4 μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0043] Preferably, the second particles coated with the lithium source in step (2) are prepared by the following method:

[0044] The second precursor and the lithium source are mixed, and then secondary calcination is performed to obtain the second particles with the surface coated with the lithium source.

[0045] Preferably, the molar ratio of lithium ions in the lithium source and the total metal ions in the second precursor is (1.05-1.1):1, but does not include 1.05:1. For example, it can be 1.06:1, 1.08:1 or 1.1:1, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable.

[0046] When preparing the second particle, the present invention ensures that the metal ions in the precursor can react completely and ensures that the surface of the second lithium particle is covered with sufficient lithium source within the above molar ratio range to provide for the formation of the nickel cobalt manganese oxide coating layer.

[0047] Preferably, a doping source is also added during the mixing of the second precursor and the lithium source, and the doping source includes any one of a zirconium source, a strontium source or a tungsten source or a combination of at least two of them, preferably a combination of a zirconium source, a strontium source and a tungsten source.

[0048] Preferably, based on the mass of the second particles of the surface-coated lithium source, the doping amount of the zirconium source is 0.08-0.20wt%, for example, it can be 0.08wt%, 0.1wt% or 0.20wt%, the doping amount of the strontium source is 0.08-0.20wt%, for example, it can be 0.08wt%, 0.1wt% or 0.20wt%, the doping amount of the tungsten source is 0.12-0.30wt%, for example, it can be 0.12wt%, 0.2wt% or 0.3wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] Preferably, the particle size of the second precursor is 1-3 μm, for example, 1 μm, 2 μm or 3 μm, and the BET is 5-10 μm. 2 / g, for example, it can be 5m 2 / g, 7m 2 / g, 9m 2 / g or 10m 2 / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] Preferably, the secondary calcination temperature is 730-930° C., such as 730° C., 830° C. or 930° C., the time is 10-30 h, such as 10 h, 20 h or 30 h, and the atmosphere is an oxygen atmosphere.

[0051] Preferably, the mass ratio of the first particles of the surface-coated cobalt-nickel compound in step (1) to the second particles of the surface-coated lithium source in step (2) is (5-9):(1-5), for example, it can be 5:5, 8:2 or 9:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] Preferably, based on the mass of the nickel cobalt aluminum oxide lithium positive electrode material, the added amount of the aluminum source is 0.08-0.32wt%, for example, it can be 0.08wt%, 0.1wt%, 0.2wt%, 0.3wt% or 0.32wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] Preferably, a doping source is also added during the mixing process in step (2). Based on the mass of the nickel cobalt aluminum oxide lithium positive electrode material, the amount of the doping source added is 0.03-0.13wt%, for example, 0.03wt%, 0.05wt%, 0.1wt% or 0.13wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] Preferably, the doping source added during the mixing process in step (2) includes any one of TiO2, CeO2, WO3, La2O3 or MgO or a combination of at least two thereof, preferably CeO2.

[0055] Preferably, the aluminum source in step (2) includes any one of Al(OH)3, Al2O3 or Al(CH3COO)3, or a combination of at least two of them.

[0056] Preferably, the sintering temperature in step (2) is 550-750°C, for example, 550°C, 600°C, 700°C or 750°C, the sintering time is 3-15h, for example, 3h, 5h, 10h or 15h, and the atmosphere is oxygen atmosphere.

[0057] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:

[0058] (1) mixing a first precursor, a lithium source and a doping source, and then calcining at a temperature of 650-800° C. for 10-30 hours in an oxygen atmosphere to obtain first particles;

[0059] The ratio of the size of the first particle in the long axis direction to the size in the short axis direction is (20-100):1, the size in the long axis direction is 5-10 μm, and the size in the short axis direction is 0.06-0.3 μm;

[0060] The doping sources are zirconium source, strontium source and tungsten source. Based on the mass of the first particles, the doping amount of the zirconium source is 0.08-0.20wt%, the doping amount of the strontium source is 0.08-0.20wt%, and the doping amount of the tungsten source is 0.12-0.35wt%;

[0061] The particle size of the first precursor is 10-17 μm, and the BET is 1-4 μm. 2 / g; the molar ratio of lithium ions in the lithium source to the total metal ions in the first precursor is (1.0-1.05):1;

[0062] (2) mixing a cobalt source, a nickel source and the first particles of step (1), and then sintering them at a temperature of 550-650° C. for 3-15 hours in an oxygen atmosphere to obtain first particles with a surface coated with a cobalt-nickel compound;

[0063] (3) mixing a second precursor, a lithium source and a doping source, and then performing secondary calcination at a temperature of 730-930° C. for 10-30 hours in an oxygen atmosphere to obtain second particles with a surface coated with the lithium source, wherein the primary particle size of the second particles with the surface coated with the lithium source is 0.5-2.4 μm;

[0064] The molar ratio of lithium ions in the lithium source to total metal ions in the second precursor is (1.05-1.1):1, but does not include 1.05:1;

[0065] The doping source includes a zirconium source, a strontium source and a tungsten source. Based on the mass of the second particles coated with the lithium source, the doping amount of the zirconium source is 0.08-0.20wt%, the doping amount of the strontium source is 0.08-0.20wt%, and the doping amount of the tungsten source is 0.12-0.30wt%;

[0066] The particle size of the second precursor is 1-3 μm, and the BET is 5-10 μm. 2 / g;

[0067] (4) mixing the aluminum source, the second particles of the lithium source coated on the surface in step (3), the first particles of the cobalt-nickel compound coated on the surface in step (2), and the doping source, and then sintering them at a temperature of 550-750° C. for 3-15 hours in an oxygen atmosphere to obtain the lithium nickel cobalt aluminum oxide positive electrode material;

[0068] The ratio of the size of the first particle in the short axis direction of step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:(6-10), and the mass ratio of the first particle coated with the cobalt-nickel compound to the second particle coated with the lithium source in step (3) is (5-9):(1-5);

[0069] Based on the mass of the nickel cobalt aluminum oxide lithium positive electrode material, the added amount of the aluminum source is 0.08-0.32wt%, and the added amount of the doping source is 0.03-0.13wt%; the doping source includes any one of TiO2, CeO2, WO3, La2O3 or MgO or a combination of at least two of them.

[0070] In a third aspect, the present invention provides a battery, comprising the lithium nickel cobalt aluminum oxide positive electrode material as described in the first aspect.

[0071] Compared with the prior art, the present invention has the following beneficial effects:

[0072] The present invention coats the surface of large particles with small particles by grading large and small particles, and matches the nickel cobalt aluminum oxide coating layer between the large and small particles, thereby improving the grading effect and bonding strength of the large and small particles, thereby further improving the cycle performance and thermal stability of the positive electrode material; at the same time, the present invention coats the surface of polycrystalline large particles with Ni source and Co source, and coats the surface of single crystal small particles with lithium source, and further sinters the polycrystalline with single crystal grading and coats Al source, so that the lithium source on the surface of the single crystal small particles further reacts with the Ni source, Co source and coating layer Al source on the surface of the polycrystalline large particles, and generates a nickel cobalt aluminum coating layer on the surface of the large and small particles, so that the small particles are tightly coated on the surface of the large particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Figure 1 This is a cross-sectional electron microscope image of the first particle in Example 1 of the present invention. DETAILED DESCRIPTION

[0074] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0075] Example 1

[0076] This embodiment provides a nickel cobalt aluminum oxide positive electrode material, the nickel cobalt aluminum oxide positive electrode material includes a first particle and a second particle coated on the surface of the first particle, and a nickel cobalt aluminum oxide coating layer is further included between the second particle and the first particle;

[0077] The first particle is a polycrystalline strip-shaped primary fiber particle, the second particle is a single crystal spherical particle, and the size of the first particle in the long axis direction is larger than the primary particle size of the second particle; the first particle and the second particle both include lithium nickel cobalt aluminum oxide, and both are doped with Zr, Sr and W elements, and the lithium nickel cobalt aluminum oxide coating layer is also doped with Ce element;

[0078] The preparation method of the lithium nickel cobalt aluminum oxide positive electrode material comprises the following steps:

[0079] (1) Add nickel, cobalt and aluminum salt solutions, sodium hydroxide solution and ammonia solution into a reactor for reaction, and then wash and dry to obtain a product with the chemical formula of Ni 0.88 Co 0.10 Al 0.02 The first precursor of (OH)2 is mixed with the first precursor, the lithium source and the doping source at a mixing speed of 1000 rpm. After mixing for 20 minutes, the mixture is calcined at 710°C for 30 hours in an oxygen atmosphere. After naturally cooling to room temperature, the material is taken out and crushed and sieved by a colloid mill to obtain the first particles. The cross-sectional electron microscope image of the first particles is shown in FIG. Figure 1 As shown;

[0080] The ratio of the size of the first particle in the long axis direction to the size in the short axis direction is 60:1, the size in the long axis direction is 8 μm, and the size in the short axis direction is 0.13 μm;

[0081] The doping sources are zirconium source, strontium source and tungsten source. Based on the mass of the first particles, the doping amount of the zirconium source is 0.1wt%, the doping amount of the strontium source is 0.1wt%, and the doping amount of the tungsten source is 0.3wt%; wherein the lithium source is lithium hydroxide, the zirconium source is ZrO2, the strontium source is SrCO3, and the tungsten source is WO3;

[0082] The particle size of the first precursor is 14 μm and the BET is 2 μm. 2 / g; the molar ratio of lithium ions in the lithium source to the total metal ions in the first precursor is 1.02:1;

[0083] (2) mixing a cobalt source, a nickel source and the first particles of step (1), and then sintering them at 550° C. for 10 h in an oxygen atmosphere to obtain first particles coated with a cobalt-nickel compound;

[0084] Based on the mass of the first particle coated with the cobalt-nickel compound, the amount of the cobalt source added is 0.16wt%, and the amount of the nickel source added is 0.16wt%, wherein the cobalt source is CoOOH and the nickel source is NiOOH;

[0085] (3) mixing a second precursor, a lithium source and a doping source at a mixing speed of 1000 rpm, and performing secondary calcination at 760° C. for 30 h in an oxygen atmosphere after mixing for 20 minutes, and then naturally cooling to room temperature and taking out the material, and air flow pulverizing and sieving to obtain second particles with a surface coated with a lithium source, wherein the primary particle size of the second particles with a surface coated with a lithium source is 1.04 μm;

[0086] The molar ratio of lithium ions in the lithium source to total metal ions in the second precursor is 1.06:1;

[0087] The doping sources are zirconium source, strontium source and tungsten source. Based on the mass of the second particles with the surface coated with lithium source, the doping amount of zirconium source is 0.1wt%, the doping amount of strontium source is 0.1wt%, and the doping amount of tungsten source is 0.30wt%; wherein the lithium source is lithium hydroxide, the zirconium source is ZrO2, the strontium source is SrCO3, and the tungsten source is WO3;

[0088] The chemical formula of the second precursor is Ni 0.88 Co 0.10 Al 0.02 (OH)2, particle size 2μm, BET 8m 2 / g;

[0089] (4) firstly mixing the second particles of the lithium source coated on the surface of step (3) and the first particles of the cobalt-nickel compound coated on the surface of step (2) to obtain a matrix, and then mixing the aluminum source, the matrix and the doping source at a mixing speed of 600 rpm. After mixing for 15 minutes, sintering at a temperature of 650° C. for 10 hours in an oxygen atmosphere, cooling naturally to room temperature, taking out the material, and sieving it to obtain the nickel cobalt aluminum oxide lithium positive electrode material;

[0090] The ratio of the size of the first particle in the short axis direction of step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:8, and the mass ratio of the first particle coated with the cobalt-nickel compound to the second particle coated with the lithium source in step (3) is 8:2;

[0091] Based on the mass of the nickel cobalt aluminum lithium positive electrode material, the added amount of the aluminum source is 0.11wt%, and the added amount of the doping source is 0.04wt%; wherein the aluminum source is Al2O3, and the doping source is CeO2.

[0092] Example 2

[0093] This embodiment provides a nickel cobalt aluminum oxide positive electrode material, the nickel cobalt aluminum oxide positive electrode material includes a first particle and a second particle coated on the surface of the first particle, and a nickel cobalt aluminum oxide coating layer is further included between the second particle and the first particle;

[0094] The first particle is a polycrystalline strip-shaped primary fiber particle, the second particle is a single crystal spherical particle, and the size of the first particle in the long axis direction is larger than the primary particle size of the second particle; the first particle and the second particle both include lithium nickel cobalt aluminum oxide, and both are doped with Zr, Sr and W elements, and the lithium nickel cobalt aluminum oxide coating layer is also doped with Ce element;

[0095] The preparation method of the lithium nickel cobalt aluminum oxide positive electrode material comprises the following steps:

[0096] (1) Add nickel, cobalt and aluminum salt solutions, sodium hydroxide solution and ammonia solution into a reactor for reaction, and then wash and dry to obtain a product with the chemical formula of Ni 0.88 Co 0.10 Al 0.02 The first precursor of (OH)2 is mixed with the first precursor, the lithium source and the doping source at a mixing speed of 1000 rpm. After mixing for 20 minutes, the mixture is calcined at 650°C for 10 hours in an oxygen atmosphere. After naturally cooling to room temperature, the material is taken out, crushed and sieved by a colloid mill to obtain the first particles.

[0097] The ratio of the size of the first particle in the long axis direction to the size in the short axis direction is 20:1, the size in the long axis direction is 5 μm, and the size in the short axis direction is 0.25 μm;

[0098] The doping sources are zirconium source, strontium source and tungsten source. Based on the mass of the first particles, the doping amount of the zirconium source is 0.08wt%, the doping amount of the strontium source is 0.08wt%, and the doping amount of the tungsten source is 0.12wt%; wherein the lithium source is lithium hydroxide, the zirconium source is ZrO2, the strontium source is SrCO3, and the tungsten source is WO3;

[0099] The particle size of the first precursor is 10 μm and the BET is 4 μm. 2 / g; the molar ratio of lithium ions in the lithium source to the total metal ions in the first precursor is 1.05:1;

[0100] (2) mixing a cobalt source, a nickel source and the first particles of step (1), and then sintering them at 650° C. for 3 h in an oxygen atmosphere to obtain first particles coated with cobalt-nickel compounds;

[0101] Based on the mass of the first particle coated with the cobalt-nickel compound, the amount of the cobalt source added is 0.32wt%, and the amount of the nickel source added is 0.32wt%, wherein the cobalt source is CoOOH and the nickel source is NiOOH;

[0102] (3) mixing a second precursor, a lithium source and a doping source at a mixing speed of 1000 rpm, and performing secondary calcination at 930° C. for 10 h in an oxygen atmosphere after mixing for 20 minutes, and then naturally cooling the mixture to room temperature and taking out the mixture, and air flow pulverizing and sieving the mixture to obtain second particles coated with the lithium source, wherein the primary particle size of the second particles coated with the lithium source is 1.5 μm;

[0103] The molar ratio of lithium ions in the lithium source to total metal ions in the second precursor is 1.1:1;

[0104] The doping sources are zirconium source, strontium source and tungsten source. Based on the mass of the second particles with the surface coated with lithium source, the doping amount of the zirconium source is 0.20wt%, the doping amount of the strontium source is 0.08wt%, and the doping amount of the tungsten source is 0.12wt%; wherein the lithium source is lithium hydroxide, the zirconium source is ZrO2, the strontium source is SrCO3, and the tungsten source is WO3;

[0105] The chemical formula of the second precursor is Ni 0.88 Co 0.10 Al 0.02 (OH)2, particle size 1 μm, BET 10m 2 / g;

[0106] (4) firstly mixing the second particles of the surface-coated lithium source in step (3) and the first particles of the surface-coated cobalt-nickel compound in step (2) to obtain a matrix, and then mixing the aluminum source, the matrix and the doping source at a mixing speed of 600 rpm. After mixing for 15 minutes, sintering at a temperature of 550° C. for 15 hours in an oxygen atmosphere, cooling naturally to room temperature, taking out the material, and sieving to obtain the nickel cobalt aluminum oxide lithium positive electrode material;

[0107] The ratio of the size of the first particle in the short axis direction of step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:6, and the mass ratio of the first particle coated with the cobalt-nickel compound to the second particle coated with the lithium source in step (3) is 5:5;

[0108] Based on the mass of the nickel cobalt aluminum lithium positive electrode material, the added amount of the aluminum source is 0.32wt%, and the added amount of the doping source is 0.13wt%; wherein the aluminum source is Al2O3, and the doping source is CeO2.

[0109] Example 3

[0110] This embodiment provides a nickel cobalt aluminum oxide positive electrode material, the nickel cobalt aluminum oxide positive electrode material includes a first particle and a second particle coated on the surface of the first particle, and a nickel cobalt aluminum oxide coating layer is further included between the second particle and the first particle;

[0111] The first particle is a polycrystalline strip-shaped primary fiber particle, the second particle is a single crystal spherical particle, and the size of the first particle in the long axis direction is larger than the primary particle size of the second particle; the first particle and the second particle both include lithium nickel cobalt aluminum oxide, and both are doped with Zr, Sr and W elements, and the lithium nickel cobalt aluminum oxide coating layer is also doped with Ce element;

[0112] The preparation method of the lithium nickel cobalt aluminum oxide positive electrode material comprises the following steps:

[0113] (1) Add nickel, cobalt and aluminum salt solutions, sodium hydroxide solution and ammonia solution into a reactor for reaction, and then wash and dry to obtain a product with the chemical formula of Ni 0.88 Co 0.10 Al 0.02 The first precursor of (OH)2 is mixed with the first precursor, the lithium source and the doping source at a mixing speed of 1000 rpm. After mixing for 20 minutes, the mixture is calcined at 800°C for 30 hours in an oxygen atmosphere. After naturally cooling to room temperature, the material is taken out, crushed and sieved by a colloid mill to obtain the first particles.

[0114] The ratio of the size of the first particle in the long axis direction to the size in the short axis direction is 100:1, the size in the long axis direction is 6 μm, and the size in the short axis direction is 0.06 μm;

[0115] The doping sources are zirconium source, strontium source and tungsten source. Based on the mass of the first particles, the doping amount of the zirconium source is 0.20wt%, the doping amount of the strontium source is 0.20wt%, and the doping amount of the tungsten source is 0.35wt%; wherein the lithium source is lithium hydroxide, the zirconium source is ZrO2, the strontium source is SrCO3, and the tungsten source is WO3;

[0116] The particle size of the first precursor is 10 μm and the BET is 4 μm. 2 / g; the molar ratio of lithium ions in the lithium source to the total metal ions in the first precursor is 1.0:1;

[0117] (2) mixing a cobalt source, a nickel source and the first particles of step (1), and then sintering them at 550° C. for 15 h in an oxygen atmosphere to obtain first particles coated with a cobalt-nickel compound;

[0118] Based on the mass of the first particle coated with the cobalt-nickel compound, the amount of the cobalt source added is 0.08wt%, and the amount of the nickel source added is 0.08wt%, wherein the cobalt source is CoOOH and the nickel source is NiOOH;

[0119] (3) mixing a second precursor, a lithium source and a doping source at a mixing speed of 1000 rpm, and performing secondary calcination at 730° C. for 30 h in an oxygen atmosphere after mixing for 20 minutes, and then naturally cooling to room temperature and taking out the material, and air flow pulverizing and sieving to obtain second particles with a surface coated with a lithium source, wherein the primary particle size of the second particles with a surface coated with a lithium source is 0.5-2.4 μm;

[0120] The molar ratio of lithium ions in the lithium source to total metal ions in the second precursor is 1.08:1;

[0121] The doping sources are zirconium source, strontium source and tungsten source. Based on the mass of the second particles with the surface coated with lithium source, the doping amount of the zirconium source is 0.08wt%, the doping amount of the strontium source is 0.08wt%, and the doping amount of the tungsten source is 0.12wt%; wherein the lithium source is lithium hydroxide, the zirconium source is ZrO2, the strontium source is SrCO3, and the tungsten source is WO3;

[0122] The chemical formula of the second precursor is Ni 0.88 Co 0.10 Al 0.02 (OH)2, particle size 1 μm, BET 10m 2 / g;

[0123] (4) firstly mixing the second particles of the surface-coated lithium source in step (3) and the first particles of the surface-coated cobalt-nickel compound in step (2) to obtain a matrix, and then mixing the aluminum source, the matrix and the doping source at a mixing speed of 600 rpm. After mixing for 15 minutes, sintering at a temperature of 750° C. for 3 hours in an oxygen atmosphere, cooling naturally to room temperature, taking out the material, and sieving to obtain the nickel cobalt aluminum oxide lithium positive electrode material;

[0124] The ratio of the size of the first particle in the short axis direction of step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:10, and the mass ratio of the first particle coated with the cobalt-nickel compound to the second particle coated with the lithium source in step (3) is 9:1;

[0125] Based on the mass of the nickel cobalt aluminum lithium positive electrode material, the added amount of the aluminum source is 0.08wt%, and the added amount of the doping source is 0.03wt%; wherein the aluminum source is Al2O3, and the doping source is CeO2.

[0126] Example 4

[0127] The present embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as the first embodiment except that in the preparation method, the doping source in step (1) is a strontium source and a tungsten source, but does not include a zirconium source, so that the size of the first particle changes accordingly, and the ratio of the size of the first particle in the short axis direction of the first particle in step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:11.

[0128] Example 5

[0129] The present embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as the first embodiment except that in the preparation method thereof, the doping source in step (1) is a zirconium source and a tungsten source, but does not include a strontium source, so that the size of the first particle changes accordingly, and the ratio of the size of the first particle in the short axis direction of the first particle in step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:11.

[0130] Example 6

[0131] The present embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as the first embodiment except that in the preparation method, the doping source in step (1) is a zirconium source and a strontium source, but does not include a tungsten source, so that the size of the first particle changes accordingly, and the ratio of the size of the first particle in the short axis direction of the first particle in step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:11.

[0132] Example 7

[0133] The present embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as that of Embodiment 1 except that in the preparation method, the doping source in step (1) is only a zirconium source, so that the size of the first particle changes accordingly, and the ratio of the size of the first particle in the short axis direction of step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:4.

[0134] Example 8

[0135] The present embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as that of Embodiment 1 except that in the preparation method, the doping source in step (1) is only a strontium source, so that the size of the first particle changes accordingly, and the ratio of the size of the first particle in the short axis direction of step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:4.

[0136] Example 9

[0137] The present embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as the first embodiment except that in the preparation method, the doping source in step (1) is only a tungsten source, so that the size of the first particle changes accordingly, and the ratio of the size of the first particle in the short axis direction of the first particle in step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:4.

[0138] Example 10

[0139] The present embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as that of embodiment 1 except that in its preparation method, the aluminum source of step (4) is added to step (2) to form first particles with a surface coated with a nickel cobalt aluminum compound, so that the obtained nickel cobalt aluminum oxide positive electrode material changes accordingly.

[0140] Embodiment 11

[0141] This embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as that of embodiment 1 except that in the preparation method, the mass of CeO2 and the like described in step (4) is replaced by TiO2, so that the obtained nickel cobalt aluminum oxide positive electrode material is changed accordingly.

[0142] Example 12

[0143] The present embodiment provides a nickel cobalt aluminum oxide positive electrode material. The nickel cobalt aluminum oxide positive electrode material is the same as that of embodiment 1 except that in the preparation method, the mass of CeO2 and the like described in step (4) is replaced by La2O3, so that the obtained nickel cobalt aluminum oxide positive electrode material is changed accordingly.

[0144] Comparative Example 1

[0145] This comparative example provides a nickel cobalt aluminum oxide positive electrode material, which is the same as Example 1 except that the first particles are spherical particles;

[0146] The preparation method of the lithium nickel cobalt aluminum oxide positive electrode material is the same as that of Example 1, except that step (1) is not doped so that the first particles are spherical particles.

[0147] Comparative Example 2

[0148] This comparative example provides a nickel cobalt aluminum oxide positive electrode material, which is the same as Example 1 except that it does not include a nickel cobalt aluminum oxide coating layer;

[0149] The method for preparing the lithium nickel cobalt aluminum oxide positive electrode material is the same as that of Example 1 except that step (2) is not performed.

[0150] The nickel cobalt aluminum oxide positive electrode materials obtained in the above embodiments and comparative examples were assembled and tested for button batteries. The specific steps of button battery production are: the positive electrode material is slurried and coated on aluminum foil. After drying, sheeting and slicing, the battery is assembled with the negative electrode, diaphragm and electrolyte in an argon-protected glove box, wherein the negative electrode is a metal lithium sheet, the diaphragm is a polyethylene (PE) microporous diaphragm, and the electrolyte is LMLiPF6-EC / DMC (volume ratio of 1:1); then the electrochemical performance test is carried out, and the test conditions are: capacity test (2.5V-4.25V, 0.2C) and 25°C cycle test (3.0V-4.5V, 0.5C / 1C), DSC test (0.1C charged to 4.3V).

[0151] The test results are shown in Table 1:

[0152] Table 1

[0153]

[0154]

[0155] From Table 1 we can see that:

[0156] The nickel cobalt aluminum oxide of the present invention has excellent cycle performance and thermal stability. It can be seen from Example 1 and Comparative Example 1 that the grading method of the present invention can improve the grading effect; it can be seen from Example 1 and Comparative Example 2 that when the nickel cobalt aluminum oxide coating layer is coated between the first particle and the second particle of the present invention, the bonding strength and grading effect of the first particle and the second particle can be improved, thereby improving the performance of the material; it can be seen from Example 1 and Examples 4-9 that the ratio of the size of the first particle in the short axis direction of the present invention to the primary particle size of the second particle will affect the grading effect of the two, thereby affecting Material properties, wherein the nickel cobalt aluminum oxide of the present invention is preferably doped with the W element, and the W element doping can further improve the material properties; it can be seen from Example 1 and Example 10 that when the nickel cobalt aluminum oxide coating layer is prepared by the present invention, it is preferred to coat the nickel cobalt compound on the surface of the first particle, and then sinter the mixed particles with the second particle coated with the lithium source and the aluminum source, which can improve the integrity of the coating layer, thereby further improving the material properties; it can be seen from Example 1 and Examples 11-12 that the nickel cobalt aluminum oxide coating layer of the present invention is preferably doped with the Ce element, and the Ce element doping can further improve the material properties.

[0157] In summary, the present invention provides a nickel cobalt aluminum oxide positive electrode material and a preparation method and application thereof. The nickel cobalt aluminum oxide positive electrode material suppresses the generation of microcracks through structural design and the matching of large and small particles, and at the same time suppresses the side reaction between the surface of the material and the electrolyte to generate a NiO rock salt phase, thereby improving the cycle performance and thermal stability of the material.

[0158] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A nickel cobalt aluminum oxide lithium positive electrode material, characterized in that: The lithium nickel cobalt aluminum oxide positive electrode material comprises a first particle and a second particle coated on the surface of the first particle, and a lithium nickel cobalt aluminum oxide coating layer is further included between the second particle and the first particle; The size of the first particle in the long axis direction is greater than the size of the second particle in the long axis direction; The first particles and the second particles both include lithium nickel cobalt aluminum oxide.

2. The nickel cobalt aluminum oxide positive electrode material according to claim 1, characterized in that: The first particles are polycrystalline strip-shaped primary fiber particles, and the second particles are single-crystal spherical particles; Preferably, the size of the first particle in the long axis direction is larger than the primary particle size of the second particle; Preferably, the first particles and the second particles are independently doped with a doping element, wherein the doping element comprises any one of Zr, Sr or W or a combination of at least two of them, preferably a combination of Zr, Sr and W; Preferably, the lithium nickel cobalt aluminum oxide coating layer is further doped with a doping element, and the doping element includes any one of Ti, Ce, W, La or Mg, or a combination of at least two of them.

3. A method for preparing the nickel cobalt aluminum oxide positive electrode material according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) mixing and sintering the first particles, the cobalt source and the nickel source to obtain the first particles with the cobalt-nickel compound coated on the surface; (2) Mixing and sintering the aluminum source and the second particles of the surface-coated lithium source with the first particles of the surface-coated cobalt-nickel compound in step (1) to obtain the nickel cobalt aluminum oxide positive electrode material.

4. The preparation method according to claim 3, characterized in that: Step (1) The ratio of the size of the first particle in the minor axis direction to the primary particle size of the second particle coated with the lithium source on the surface is 1:(6-10); Preferably, in step (1), the ratio of the size of the first particle in the long axis direction to the size of the first particle in the short axis direction is (20-100):1; Preferably, in step (1), the first particles have a size of 5-10 μm in the long axis direction and a size of 0.06-0.3 μm in the short axis direction.

5. The preparation method according to claim 4, characterized in that: Step (1) The first particles are prepared by the following method: Mixing a first precursor and a lithium source, and then calcining once to obtain the first particles; Preferably, a doping source is also added during the mixing of the first precursor and the lithium source, and the doping source includes any one of a zirconium source, a strontium source or a tungsten source, or a combination of at least two of them, preferably a combination of a zirconium source, a strontium source and a tungsten source; Preferably, based on the mass of the first particles, the doping amount of the zirconium source is 0.08-0.20wt%, the doping amount of the strontium source is 0.08-0.20wt%, and the doping amount of the tungsten source is 0.12-0.35wt%; Preferably, the particle size of the first precursor is 10-17 μm, and the BET is 1-4 μm. 2 / g; Preferably, the molar ratio of lithium ions in the lithium source to total metal ions in the first precursor is (1.0-1.05):1; Preferably, the primary calcination is carried out at a temperature of 650-800° C., for a time of 10-30 hours, in an oxygen atmosphere.

6. The preparation method according to claim 4 or 5, characterized in that: The sintering temperature in step (1) is 550-650° C., the sintering time is 3-15 hours, and the atmosphere is an oxygen atmosphere; Preferably, the cobalt source in step (1) comprises any one or a combination of at least two of Co3O4, CoOOH, Co(OH)2 or CoCO3; Preferably, the nickel source in step (1) comprises any one of NiOOH, Ni(OH)2, NiCO3 or NiO, or a combination of at least two thereof; Preferably, based on the mass of the first particles of the surface-coated cobalt-nickel compound in step (1), the amount of the cobalt source added in step (1) is 0.08-0.32 wt%, and the amount of the nickel source added in step (1) is 0.08-0.32 wt%.

7. The preparation method according to any one of claims 4 to 6, characterized in that: The primary particle size of the second particles coated with the lithium source in step (2) is 0.5-2.4 μm; Preferably, the second particles coated with the lithium source in step (2) are prepared by the following method: Mixing a second precursor and a lithium source, and then performing secondary calcination to obtain second particles with the surface coated with the lithium source; Preferably, the molar ratio of lithium ions in the lithium source to the total metal ions in the second precursor is (1.05-1.1):1, but does not include 1.05:1; Preferably, a doping source is also added during the mixing of the second precursor and the lithium source, and the doping source includes any one of a zirconium source, a strontium source or a tungsten source, or a combination of at least two of them, preferably a combination of a zirconium source, a strontium source and a tungsten source; Preferably, based on the mass of the second particles coated with the lithium source, the doping amount of the zirconium source is 0.08-0.20wt%, the doping amount of the strontium source is 0.08-0.20wt%, and the doping amount of the tungsten source is 0.12-0.30wt%; Preferably, the particle size of the second precursor is 1-3 μm, and the BET is 5-10 μm. 2 / g; Preferably, the secondary calcination is carried out at a temperature of 730-930° C., for a time of 10-30 h, in an oxygen atmosphere.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The mass ratio of the first particles of the surface coated with the cobalt-nickel compound in step (1) to the second particles of the surface coated with the lithium source in step (2) is (5-9):(1-5); Preferably, based on the mass of the nickel cobalt aluminum oxide lithium positive electrode material, the added amount of the aluminum source is 0.08-0.32wt%; Preferably, a doping source is also added during the mixing process in step (2), and the amount of the doping source added is 0.03-0.13 wt % based on the mass of the lithium nickel cobalt aluminum oxide positive electrode material; Preferably, the doping source added in the mixing process of step (2) includes any one of TiO2, CeO2, WO3, La2O3 or MgO, or a combination of at least two thereof; Preferably, the sintering temperature in step (2) is 550-750° C., the sintering time is 3-15 hours, and the atmosphere is an oxygen atmosphere.

9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises the following steps: (1) mixing a first precursor, a lithium source and a doping source, and then calcining at a temperature of 650-800° C. for 10-30 hours in an oxygen atmosphere to obtain first particles; The ratio of the size of the first particle in the long axis direction to the size in the short axis direction is (20-100):1, the size in the long axis direction is 5-10 μm, and the size in the short axis direction is 0.06-0.3 μm; The doping sources are zirconium source, strontium source and tungsten source. Based on the mass of the first particles, the doping amount of the zirconium source is 0.08-0.20wt%, the doping amount of the strontium source is 0.08-0.20wt%, and the doping amount of the tungsten source is 0.12-0.35wt%; The particle size of the first precursor is 10-17 μm, and the BET is 1-4 μm. 2 / g; the molar ratio of lithium ions in the lithium source to the total metal ions in the first precursor is (1.0-1.05):1; (2) mixing a cobalt source, a nickel source and the first particles of step (1), and then sintering them at a temperature of 550-650° C. for 3-15 hours in an oxygen atmosphere to obtain first particles with a surface coated with a cobalt-nickel compound; (3) mixing a second precursor, a lithium source and a doping source, and then performing secondary calcination at a temperature of 730-930° C. for 10-30 hours in an oxygen atmosphere to obtain second particles with a surface coated with the lithium source, wherein the primary particle size of the second particles with the surface coated with the lithium source is 0.5-2.4 μm; The molar ratio of lithium ions in the lithium source to total metal ions in the second precursor is (1.05-1.1):1, but does not include 1.05:1; The doping source comprises a zirconium source, a strontium source and a tungsten source. Based on the mass of the second particles coated with the lithium source, the doping amount of the zirconium source is 0.08-0.20wt%, the doping amount of the strontium source is 0.08-0.20wt%, and the doping amount of the tungsten source is 0.12-0.30wt%; The particle size of the second precursor is 1-3 μm, and the BET is 5-10 μm. 2 / g; (4) mixing the aluminum source, the second particles of the lithium source coated on the surface in step (3), the first particles of the cobalt-nickel compound coated on the surface in step (2), and the doping source, and then sintering them at a temperature of 550-750° C. for 3-15 hours in an oxygen atmosphere to obtain the lithium nickel cobalt aluminum oxide positive electrode material; The ratio of the size of the first particle in the short axis direction of step (1) to the primary particle size of the second particle coated with the lithium source in step (3) is 1:(6-10), and the mass ratio of the first particle coated with the cobalt-nickel compound to the second particle coated with the lithium source in step (3) is (5-9):(1-5); Based on the mass of the nickel cobalt aluminum oxide lithium positive electrode material, the added amount of the aluminum source is 0.08-0.32wt%, and the added amount of the doping source is 0.03-0.13wt%; the doping source includes any one of TiO2, CeO2, WO3, La2O3 or MgO or a combination of at least two of them.

10. A battery, characterized in that: The battery comprises the lithium nickel cobalt aluminum oxide positive electrode material as described in any one of claims 1 to 3.

Citation Information

Cited By

  • Positive electrode material and preparation method thereof, positive plate and secondary battery

    CN120933346A