ZrN film aqueous zinc-based battery negative electrode material and preparation method and application thereof
By using plasma enhanced atomic layer deposition technology in zinc ion batteries, the problem of zinc dendrites is solved, the cycle stability and safety of the battery are improved, and high conductivity and corrosion resistance are maintained.
Patent Information
- Application Number
- CN202411298536.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-03
AI Technical Summary
Zinc ion batteries are prone to form zinc dendrites during charging and discharging, resulting in a shortening of battery life and safety risks. It is difficult for the prior art to effectively inhibit its growth.
A ZrN film is deposited on the surface of metal zinc sheets by plasma-enhanced atomic layer deposition technology. By controlling the content and number of cycles of N2/H2 mixed gas, a dense and uniform ZrN film is formed to prevent the growth of zinc dendrites.
It significantly improves the electrochemical performance and cycle stability of zinc ion batteries, extends the battery life, and improves safety, while maintaining high conductivity and corrosion resistance.
Smart Images

Figure CN119069679A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of zinc-based batteries and relates to a ZrN thin film aqueous zinc-based battery negative electrode material and a preparation method and application thereof. Background Art
[0002] With the growing global demand for clean energy and the continuous advancement of sustainable development goals, the research on new energy storage technologies has become a hot topic in the international scientific community. Among the many energy storage solutions, aqueous zinc-ion batteries (AZIBs) have attracted widespread attention due to their environmentally friendly characteristics, low cost and high safety. Compared with traditional lithium-ion batteries, zinc-ion batteries use zinc, which is abundant on the earth and relatively cheap, as the negative electrode material, which not only helps to reduce production costs, but also reduces dependence on scarce resources. In addition, zinc-ion batteries also have a higher theoretical specific capacity, which means that they can store more energy, thus showing great potential in large-scale energy storage applications, such as grid energy storage, electric vehicle batteries and other fields.
[0003] However, the development of zinc-ion batteries has not been smooth sailing. A significant technical obstacle is that the zinc negative electrode is prone to form so-called "zinc dendrites" during the charge and discharge process. This slender metal structure will gradually grow during the battery cycle and may penetrate the separator inside the battery, causing an internal short circuit, greatly shortening the battery's service life and increasing potential safety risks. Therefore, inhibiting the growth of zinc dendrites has become a key technical challenge to improve the performance of zinc-ion batteries.
[0004] In order to overcome this problem, researchers have conducted explorations in many aspects. A common method is to coat the zinc negative electrode with a layer of inorganic or organic material through surface modification technology to enhance its stability and conductivity. Other researchers have tried to use alloying technology to change the chemical composition of the zinc negative electrode to improve its electrochemical behavior. Although these methods have achieved certain success under laboratory conditions, they still face many challenges in practical applications. For example, the electrochemical stability of the coating material is often insufficient and difficult to maintain in long-term cycles; in addition, the conductivity of the coating material is also a problem that needs to be solved, because poor conductivity will affect the overall performance of the battery; furthermore, the uniformity and controllability of the coating thickness are also important factors affecting its effect.
[0005] Although aqueous zinc-ion batteries have many advantages in theory, their widespread commercial application still requires breakthroughs in key technologies such as zinc dendrite suppression. In the future, with the application of more innovative technologies and advances in materials science, zinc-ion batteries are expected to become an important part of the clean energy transition. Summary of the invention
[0006] The purpose of the present invention is to solve the above problems in the prior art and propose a ZrN thin film aqueous zinc-based battery negative electrode material to improve the electrochemical performance and cycle stability of the aqueous zinc ion battery negative electrode.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] A ZrN thin film aqueous zinc-based battery negative electrode material, wherein the negative electrode material deposits ZrN with a thickness of 50-210 nm on the surface of a metal zinc sheet by plasma enhanced atomic layer deposition.
[0009] As a preferred embodiment, the negative electrode material is deposited on the surface of the metal zinc sheet by plasma enhanced atomic layer deposition with a thickness of 110 nm ZrN.
[0010] The present invention also provides a method for preparing the above-mentioned ZrN thin film aqueous zinc-based battery negative electrode material, the method comprising the following steps: placing a pretreated metal zinc sheet in a plasma enhanced atomic layer deposition chamber, using tetramethylammonium zirconium as a zirconium source and N2 / H2 mixed gas as a nitrogen source, performing cyclic growth at 250-350°C, and purging with argon gas.
[0011] In the above-mentioned method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material, the pretreatment includes grinding, polishing and alcohol cleaning.
[0012] In the above-mentioned method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material, the volume content of H2 in the N2 / H2 mixed gas is 10% to 15%. H2 mainly plays the role of a reducing agent in the mixed gas, which can effectively reduce the zirconium source in tetramethylammonium zirconium and promote the formation of the film. The present invention controls the volume content of H2 in the N2 / H2 mixed gas to be between 10% and 15%, which can improve the nitridation reaction efficiency of the ZrN film while ensuring the reduction effect, and form a dense and uniform film, wherein too high H2 content may generate hydrides or cause film defects, and too low H2 content will result in insufficient reduction effect, affecting the film quality. The present invention can ensure that the ZrN film has excellent conductivity and mechanical stability by reasonably controlling the H2 content, thereby improving the electrochemical performance and cycle life of the zinc-based battery.
[0013] In the above-mentioned method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material, the number of cycles in the cyclic growth process is 350-1400 times. The present invention controls the film thickness by controlling the number of cycles. If the number of cycles is too small, the film will be too thin, and the film may not be able to form a complete and dense covering layer, and it will not be able to effectively inhibit the growth of zinc dendrites and improve the corrosion resistance of the electrode, thereby affecting the cycle stability of the zinc-based battery. On the contrary, if the number of cycles is too large, resulting in the film being too thick, it may increase the internal stress of the film, reduce the conductivity of the electrode, and increase the volume of the electrode, thereby affecting the energy density and rate performance of the battery.
[0014] In the above-mentioned method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material, each cycle in the cyclic growth process consists of tetramethylammonium zirconium release, argon first purge, plasma pulse excitation of N2 / H2 mixed gas, and argon second purge. In the cyclic growth process of ZrN film, the role of blowing argon twice is mainly to ensure the sufficiency of the reaction and the quality of the film. The role of the first argon purge is to remove unreacted precursors and by-products in the reaction chamber after the release of tetramethylammonium zirconium to prevent their residues from interfering with subsequent reactions. The second argon purge is carried out after the plasma pulse excites the N2 / H2 mixed gas, with the purpose of removing excess gas molecules and plasma by-products, ensuring that each layer of ZrN film is evenly and densely deposited, thereby improving the quality of the film and the controllability of growth.
[0015] In the above-mentioned method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material, the growth thickness of the ZrN thin film in each cycle during the cyclic growth process is 0.1-0.2 nanometers.
[0016] In the above-mentioned method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material, the growth thickness of the ZrN thin film in each cycle during the cyclic growth process is 0.1375 nanometers.
[0017] The present invention also provides an aqueous zinc ion battery, which comprises the above-mentioned negative electrode material or the negative electrode material prepared by the above-mentioned method.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The present invention uses E-ALD technology to precisely control the ZrN film at the atomic level, thereby ensuring the uniformity and density of the coating. This uniform and dense ZrN coating can form a solid protective barrier on the surface of the zinc negative electrode, effectively preventing the growth of zinc dendrites and avoiding the internal short circuit of the battery caused by the presence of zinc dendrites, thereby greatly improving the cycle life and safety of the battery;
[0020] 2. The ultra-thin structure of the ZrN film of the present invention enables it to significantly improve the performance of the electrode without negatively affecting the overall volume capacity of the battery. This is because the thickness of the film is very small and almost does not take up additional space, thus ensuring the energy density of the battery at the same volume. In addition, this ultra-thin coating can also effectively improve the interface contact of the zinc negative electrode, promote ion transmission, and further enhance the overall performance of the battery;
[0021] 3. The ZrN film of the present invention not only has high conductivity, but also has excellent corrosion resistance. The combination of the two enables the aqueous zinc ion battery to maintain stable electrochemical performance after a long period of charge and discharge cycles. High conductivity means that electrons can pass through the coating more quickly, reducing energy loss inside the battery; while excellent corrosion resistance ensures that the coating is durable in harsh electrochemical environments and is not prone to degradation or peeling. These two characteristics work together to enable the battery to maintain high energy efficiency and a long service life even after long-term use. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a scanning electron microscope (SEM) image of the ZrN coating on the surface of the negative electrode zinc foil prepared in Example 1 with a thickness of 55 nm.
[0023] Figure 2 This is a scanning electron microscope (SEM) image of the negative electrode zinc foil of Comparative Example 1.
[0024] Figure 3 This is a high-resolution X-ray photoelectron spectroscopy (XPS) graph of Zr and N elements in the ZrN coating prepared in Example 1.
[0025] Figure 4 The cycle performance of the symmetrical batteries assembled according to Example 2 is shown in Example 1, Comparative Example 2 and Comparative Example 3.
[0026] Figure 5 The cross-sectional thickness of Example 1 was obtained by sampling with a focused ion beam (FIB) and photographed with a transmission electron microscope. The thickness was 110 nm.
[0027] Figure 6 Symmetric cells were assembled with the negative electrode materials of Example 1 and Comparative Example 1 at room temperature and at 5 mA cm -2 , 1mAh cm -2 Cycling performance of aqueous zinc-ion symmetric batteries under conditions of .
[0028] Figure 7 Symmetric cells were assembled with the negative electrode materials of Example 1 and Comparative Example 1 at room temperature. -2 , 1mAh cm -2Cycling performance of aqueous zinc-ion symmetric batteries under conditions of .
[0029] Figure 8 The negative electrode materials of Example 1 and Comparative Example 1 were assembled into a symmetrical battery at room temperature, and the current was 1-15 mA cm -2 , 1mAhcm -2 The rate performance of aqueous zinc-ion symmetric batteries under conditions of .
[0030] Fig. 9 The Tafel curves of the symmetrical batteries assembled with the negative electrode materials of Example 1 and Comparative Example 1 at room temperature were measured by an electrochemical station.
[0031] Fig.10 LSV curves of symmetrical batteries assembled with the negative electrode materials of Example 1 and Comparative Example 1 measured by an electrochemical station at room temperature. DETAILED DESCRIPTION
[0032] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.
[0033] In some embodiments of the present invention, the aluminum alloy comprises the following components in mass percentage:
[0034] Embodiment 1:
[0035] S1. Use commercial zinc foil as the substrate, first grind and polish it to remove the surface oxide layer and impurities. Use 2000 sandpaper to grind the zinc foil, then use anhydrous ethanol and deionized water ultrasonic cleaning for 5 minutes each. The cleaned zinc foil is vacuum dried at 70℃.
[0036] S2. Place the pretreated zinc foil into the vacuum chamber of the PE-ALD equipment to deposit the ZrN ultra-thin film.
[0037] During the deposition process, tetramethylammonium zirconium (TDMZ) was used as the zirconium source and N2 / H2 mixed gas was used as the nitrogen source.
[0038] Deposition temperature: The temperature of the reaction chamber was maintained at 300 °C.
[0039] S3. Tetramethylammonium zirconium (TDMZ) is introduced into the cavity with a pulse time of 0.5 seconds, followed by argon purge for 5 seconds, and then N2 / H2 mixed gas (with H2 volume content of 13%) is introduced to excite plasma with a power of 300W, react for 1 second, and then argon purge is performed again for 5 seconds.
[0040] S4. The film thickness is precisely controlled by controlling the number of cycles of step S3. In this embodiment, 800 cycles are performed to finally obtain a ZrN film with a thickness of 110 nanometers.
[0041] The morphology of the deposited ZrN film was observed using a scanning electron microscope (SEM), and the results showed that the ZrN coating was evenly and densely covered on the surface of the zinc foil. Elemental analysis was performed using X-ray photoelectron spectroscopy (XPS), confirming the successful incorporation of Zr and N elements. The film thickness was measured using a TEM cross-section after the sample was treated with a focused ion beam (FIB), confirming that the thickness of the ZrN film was 110 nanometers.
[0042] Embodiment 2:
[0043] S1. Use commercial zinc foil as the substrate, first grind and polish it to remove the surface oxide layer and impurities. Use 2000 sandpaper to grind the zinc foil, then use anhydrous ethanol and deionized water ultrasonic cleaning for 5 minutes each. The cleaned zinc foil is vacuum dried at 70℃.
[0044] S2. Place the pretreated zinc foil into the vacuum chamber of the PE-ALD equipment to deposit the ZrN ultra-thin film.
[0045] During the deposition process, tetramethylammonium zirconium (TDMZ) was used as the zirconium source and N2 / H2 mixed gas was used as the nitrogen source.
[0046] Deposition temperature: The temperature of the reaction chamber was maintained at 300 °C.
[0047] S3. Tetramethylammonium zirconium (TDMZ) is introduced into the cavity with a pulse time of 0.5 seconds, followed by argon purge for 5 seconds, and then N2 / H2 mixed gas (with H2 volume content of 13%) is introduced to excite plasma with a power of 300W, react for 1 second, and then argon purge is performed again for 5 seconds.
[0048] S4. The film thickness is precisely controlled by controlling the number of cycles of step S3. In this embodiment, 400 cycles are performed to finally obtain a ZrN film with a thickness of 55 nanometers.
[0049] Embodiment 3:
[0050] S1. Use commercial zinc foil as the substrate, first grind and polish it to remove the surface oxide layer and impurities. Use 2000 sandpaper to grind the zinc foil, then use anhydrous ethanol and deionized water ultrasonic cleaning for 5 minutes each. The cleaned zinc foil is vacuum dried at 70℃.
[0051] S2. Place the pretreated zinc foil into the vacuum chamber of the PE-ALD equipment to deposit the ZrN ultra-thin film.
[0052] During the deposition process, tetramethylammonium zirconium (TDMZ) was used as the zirconium source and N2 / H2 mixed gas was used as the nitrogen source.
[0053] Deposition temperature: The temperature of the reaction chamber was maintained at 300 °C.
[0054] S3. Tetramethylammonium zirconium (TDMZ) is introduced into the cavity with a pulse time of 0.5 seconds, followed by argon purge for 5 seconds, and then N2 / H2 mixed gas (with H2 volume content of 13%) is introduced to excite plasma with a power of 300W, react for 1 second, and then argon purge is performed again for 5 seconds.
[0055] S4. The film thickness is precisely controlled by controlling the number of cycles of step S3. In this embodiment, 1500 cycles are performed to finally obtain a ZrN film with a thickness of 206.25 nanometers.
[0056] Comparative Example 1:
[0057] Ordinary commercial zinc foil without plasma-enhanced atomic layer deposition.
[0058] Comparative Example 2:
[0059] The only difference from Example 1 is that the thickness of the ZrN coating on the surface of the negative electrode zinc foil is 10 nm.
[0060] Comparative Example 3:
[0061] The only difference from Example 1 is that the thickness of the ZrN coating on the surface of the negative electrode zinc foil is 250 nm.
[0062] The ZrN-coated zinc foils prepared in Examples 1-3 and Comparative Examples 1-3 were used as the two end electrodes of the symmetrical battery, zinc foils of the same size were used as the negative electrode and the positive electrode, and the electrolyte was a 2M ZnSO4 solution, to assemble a CR2032 button symmetrical battery.
[0063] The symmetrical battery was subjected to long-term charge and discharge cycle tests in constant current mode, and 1mAh cm-2 was charged and discharged at current densities of 1mA cm-2 and 5mA cm-2, respectively. At a current density of 1mA cm-2, after 1200h of cycling, the symmetrical battery was still able to maintain a stable voltage platform without obvious voltage hysteresis, indicating that the ZrN-modified zinc negative electrode has excellent cycle stability. At a current density of 5mA cm-2, a 5000h cycle test was carried out, and the results showed that the battery's voltage platform remained stable, and there was no obvious voltage fluctuation or dendrite short-circuiting phenomenon.
[0064] The rate performance tests were carried out at different current densities from 1mA cm-2 to 15mA cm-2. The results showed that the symmetrical cell with ZrN coating can still maintain stable electrochemical performance at high current density (15mA cm-2) with small voltage polarization. Compared with the unmodified zinc foil, the ZrN-modified zinc anode showed better voltage stability and lower voltage polarization under high rate conditions.
[0065] Figure 1 This is a scanning electron microscope (SEM) image of the ZrN coating with a thickness of 55 nm on the surface of the negative electrode zinc foil prepared in Example 1. It can be seen from the figure that the ZrN coating is uniformly deposited on the surface of the zinc foil, and the surface is relatively smooth and dense, without obvious holes or cracks, showing the superiority of PE-ALD technology in controlling coating thickness and uniformity.
[0066] Figure 2 This is a scanning electron microscope (SEM) image of the negative zinc foil of Comparative Example 1. As can be seen from the figure, the surface of the unmodified negative zinc foil is relatively rough, with significant bumps and cracks, and there are obviously more surface defects, which may lead to the rapid growth of zinc dendrites and the decline of electrode performance.
[0067] Figure 3 This is a high-resolution X-ray photoelectron spectroscopy (XPS) diagram of Zr and N elements in the ZrN coating prepared in Example 1. As can be seen from the figure, the characteristic peaks of Zr and N are clearly visible, indicating that the chemical composition purity of the ZrN coating is high. The binding energy positions of Zr 3d and N1s confirm that Zr and N in the coating are combined in the form of ZrN, further verifying that the ZrN coating was successfully prepared.
[0068] Figure 4 The cycle performance of the symmetrical battery assembled according to Example 2 is shown in Example 1, Comparative Example 2, and Comparative Example 3. As can be seen from the figure, the battery cycle performance of Example 1 is significantly better than that of the batteries of Comparative Example 2 and Comparative Example 3, showing higher cycle stability and lower capacity decay, indicating that the ZrN coating effectively inhibits the growth of zinc dendrites and prolongs the service life of the battery.
[0069] Figure 5 The cross-sectional thickness of Example 1 photographed by transmission electron microscopy after sample preparation by focused ion beam (FIB) is 110 nm. As can be seen from the figure, the ZrN coating has uniform thickness, and no obvious interlayer defects or discontinuities are found in the entire coating, further verifying that the ZrN coating prepared by the PE-ALD process has good structural integrity.
[0070] Figure 6 Symmetric cells were assembled with the negative electrode materials of Example 1 and Comparative Example 1 at room temperature and at 5 mA cm -2 , 1mAh cm -2The cycling performance of aqueous zinc ion symmetric battery under the condition of . As can be seen from the figure, the battery of Example 1 still maintains good cycling stability at high current density, while the battery performance of Comparative Example 1 decays rapidly, indicating that the ZrN coating significantly improves the durability and stability of the electrode.
[0071] Figure 7 Symmetric cells were assembled with the negative electrode materials of Example 1 and Comparative Example 1 at room temperature. -2 , 1mAh cm -2 The cycle performance of aqueous zinc ion symmetric battery under the condition of . As can be seen from the figure, the battery of Example 1 also shows better cycle performance at a lower current density, and the battery of Comparative Example 1 shows obvious performance degradation after dozens of cycles.
[0072] Figure 8 The negative electrode materials of Example 1 and Comparative Example 1 were assembled into a symmetrical battery at room temperature, and the current was 1-15 mA cm -2 , 1mAhcm -2 The rate performance of aqueous zinc ion symmetric battery under the condition of . As can be seen from the figure, the battery of Example 1 shows good rate performance at different current densities, and the battery capacity remains relatively stable with the increase of current density, while the capacity of the battery of Comparative Example 1 drops sharply at a higher current density, indicating that the ZrN coating significantly improves the rate performance of the electrode.
[0073] Fig. 9 The Tafel curves of the symmetrical cells assembled with the negative electrode materials of Example 1 and Comparative Example 1 at room temperature were measured by an electrochemical station. As can be seen from the figure, the corrosion current density of Example 1 is also significantly lower than that of Comparative Example 1, indicating that the ZrN coating has an inhibitory effect on the corrosion of the negative electrode.
[0074] Fig.10 The LSV curves of the symmetrical battery assembled with the negative electrode materials of Example 1 and Comparative Example 1 at room temperature were measured by an electrochemical station. As can be seen from the figure, the hydrogen evolution performance of Example 1 is better than that of Comparative Example 1, indicating that the ZrN film has a significant effect of inhibiting the hydrogen evolution reaction.
[0075] The capacity of the battery in Comparative Examples 2-3 decays rapidly during the cycle, and in the rate performance test, the capacity decreases significantly with the increase of current density, mainly because the unmodified zinc negative electrode cannot effectively inhibit the growth of zinc dendrites and surface corrosion. Although the battery performance of Examples 2-3 has improved, it is still not as good as that of Example 1. The cycle stability and rate performance are relatively excellent, indicating that the optimization of the ZrN coating still needs to be further improved.
[0076] In summary, the present invention uses E-ALD technology to precisely control the ZrN film at the atomic level, thereby ensuring the uniformity and density of the coating. This uniform and dense ZrN coating can form a solid protective barrier on the surface of the zinc negative electrode, effectively preventing the growth of zinc dendrites, and avoiding the internal short circuit of the battery caused by the presence of zinc dendrites, thereby greatly improving the cycle life and safety of the battery. The ultra-thin structure of the ZrN film of the present invention enables it to significantly improve the performance of the electrode without having a negative impact on the overall volume capacity of the battery. This is because the thickness of the film is very small and almost no additional space is taken up, thereby ensuring the energy density of the battery at the same volume. In addition, this ultra-thin coating can also effectively improve the interface contact of the zinc negative electrode, promote ion transmission, and further enhance the overall performance of the battery.
[0077] The parts of the embodiments herein that are not exhaustive of the midpoint values of the technical scope claimed for protection by the present invention and the new technical solutions formed by equivalent replacement of single or multiple technical features in the technical solutions of the embodiments are also within the scope claimed for protection by the present invention; at the same time, in all the listed or unlisted embodiments of the scheme of the present invention, each parameter in the same embodiment merely represents an example of its technical solution (i.e., a feasible solution), and there is no strict coordination and limitation relationship between the parameters, wherein the parameters can be replaced with each other without violating the axioms and the claims of the present invention, unless otherwise stated.
[0078] The technical means disclosed in the scheme of the present invention are not limited to the technical means disclosed in the above technical means, but also include technical schemes composed of any combination of the above technical features. The above is a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also regarded as the protection scope of the present invention.
[0079] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A ZrN thin film aqueous zinc-based battery negative electrode material, characterized in that: The negative electrode material is prepared by depositing ZrN with a thickness of 50-210 nm on the surface of a metal zinc sheet through plasma enhanced atomic layer deposition.
2. A method for preparing the ZrN thin film aqueous zinc-based battery negative electrode material as claimed in claim 1, characterized in that: The method comprises the following steps: placing a pretreated metal zinc sheet in a plasma enhanced atomic layer deposition chamber, using tetramethylammonium zirconium as a zirconium source and N2 / H2 mixed gas as a nitrogen source, performing cyclic growth at 250-350° C., and purging with argon gas.
3. The method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material according to claim 2, characterized in that: Pretreatment includes grinding, polishing and alcohol cleaning.
4. The method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material according to claim 2, characterized in that: The volume content of H2 in the N2 / H2 mixed gas is 10% to 15%.
5. The method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material according to claim 2, characterized in that: The number of cycles during the cyclic growth process ranges from 350 to 1400.
6. The method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material according to claim 2, characterized in that: Each cycle in the cyclic growth process consists of tetramethylammonium zirconium release, a first argon purge, plasma pulse excitation of N2 / H2 mixed gas, and a second argon purge.
7. The method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material according to claim 2, characterized in that: During the cyclic growth process, the growth thickness of the ZrN film is 0.1-0.2 nanometers in each cycle.
8. The method for preparing a ZrN thin film aqueous zinc-based battery negative electrode material according to claim 2, characterized in that: During the cyclic growth process, the growth thickness of the ZrN film is 0.1375 nanometers in each cycle.
9. An aqueous zinc ion battery, characterized in that: The aqueous zinc ion battery comprises the negative electrode material according to claim 1 or the negative electrode material prepared by the method according to claims 2-8.
Citation Information
Cited By
Secondary battery, preparation method therefor and electrical device
WO2026175012A1