Laminated battery and method for manufacturing laminated battery
A laminated battery with a welded portion featuring multiple angled bends facing the electrode body enhances impact resistance, addressing the vulnerability of welded portions to external impacts and maintaining battery integrity.
Patent Information
- Application Number
- CN202410676246.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-03
AI Technical Summary
Laminated batteries face issues with impact resistance, as the welded portions of the laminate film can be damaged by external impacts, affecting battery performance.
The laminated battery design incorporates a welded portion with multiple bends, including angles less than 90° and one top bend less than 180°, with at least a portion of the weld facing the electrode body, enhancing impact resistance by allowing the weld to deform against the electrode body.
The design improves the impact resistance of the welded portions, preventing damage to the electrode body by absorbing external impacts and maintaining battery performance.
Smart Images

Figure CN119069770A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a laminated battery and a method of manufacturing the laminated battery. Background Art
[0002] In a laminated battery in which an electrode body is covered with a laminate film, a portion of the laminate film is welded to form a welded portion in order to seal the electrode body.
[0003] For example, Japanese Patent Publication No. 2019-200973 discloses a method for manufacturing a secondary battery, wherein the secondary battery has a bent portion at at least one end in an outer body that has been subjected to a lamination process, and the manufacturing method comprises: a process of bringing a pressing plate into contact with a base point of the bending of the end of the outer body; and after the contact process, sliding the pressing plate and a pressing plate arranged at a position opposite to the pressing plate in a manner of clamping the end, bending the end around the base point, and forming the bent portion by clamping the end by the pressing plate and the pressing plate, wherein the surface that slides with the end of the pressing plate has an inclined surface for bending the end and a clamping surface for clamping the end, the inclined surface is inclined in a manner that narrows the cross-sectional area of the pressing plate in the sliding direction on a cross section orthogonal to the width direction of the pressing plate, and the inclined surface is inclined in the width direction. Summary of the invention
[0004] In a laminated battery in which an electrode body is covered with a single laminate film, a welded portion is formed by overlapping one end side and the other end side of the laminate film and fusing the inner surfaces thereof, thereby enclosing the electrode body through the laminate film. In addition, in a laminated battery in which an electrode body is covered with a plurality of laminate films, a welded portion is formed by overlapping the ends of the plurality of laminate films and fusing the inner surfaces thereof, thereby enclosing. Furthermore, in order to improve the structural efficiency of the laminated battery, for example, these welded portions are bent to reduce the overall external dimensions of the laminated battery.
[0005] Here, when an impact is applied to an electrode body included in a laminated battery, the electrode body may be damaged, and the required battery performance may not be achieved. Therefore, impact resistance is required for laminated batteries, and even the welded portion of the laminate film is required to have improved impact resistance to impacts applied from the outside.
[0006] The present disclosure has been made in view of the above-mentioned situation, and an object of the present disclosure is to provide a laminated battery having a weld portion having excellent impact resistance against external impact, and a method for manufacturing the laminated battery.
[0007] <1>
[0008] A laminated battery having:
[0009] Electrode body, and
[0010] a laminate film covering the electrode body and sealing it inside,
[0011] The laminate film has a welded portion where the ends overlap each other and the inner surfaces are welded together,
[0012] The welded portion has three or more bends, the three or more bends include two or more bends bent at an angle of less than 90° into an angle or an arc, and a top end side bend bent at an angle of less than 180° at the top end of the welded portion into an angle or an arc.
[0013] The weld portion has a shape in which at least a portion of a tip thereof faces the electrode body.
[0014] <2>
[0015] According to the laminated battery described in <1>, the bent portion and the front end side bent portion are both bent in an arc shape.
[0016] <3>
[0017] according to <1> or <2> In the laminated battery, the position where the tip-side bent portion is arranged is the position closest to the bent portion closest to the root side of the welded portion among the two or more bent portions.
[0018] <4>
[0019] according to <1> ~ <3> In any one of the laminated batteries, the welded portion has as the bent portion: one or more right-angled bent portions bent at an angle of 70° to 90°, and one folded-back bent portion bent at an angle of 20° or less.
[0020] <5>
[0021] according to <1> ~ <4> In the laminated battery described in any one of the above, the shortest distance between the tip of the weld and the laminate film covering the region of the electrode body is 0.5 mm to 5 mm.
[0022] <6>
[0023] A method for manufacturing a laminated battery as described in <5>, comprising:
[0024] A step of preparing a welded laminated battery having a planar welded portion formed by overlapping the ends of the laminated films and welding the inner surfaces thereof;
[0025] a folding and bending step of forming a folded and bent portion in which the fused portion in the fused laminated battery is bent at an angle of 20° or less into an angular or arc shape; and
[0026] The right-angle bending step is to form a right-angled bent portion bent into an angle or an arc shape at an angle of 70° or more and 90° or less in a region closer to the root side of the weld portion than the folded-back bent portion.
[0027] The right-angle bending step is a step of bending the welded portion in stages to form the right-angle bent portion by conveying between each pair of rollers in a roller pair group, wherein the roller pair group comprises: at least three bending rollers in contact with the surface of the bending side of the welded portion and having different contact angles with respect to the welded portion, and opposing rollers provided at positions opposing the bending rollers across the welded portion and having the same number as the bending rollers;
[0028] Furthermore, the right-angle bending step is a step of causing a region on the front end side of the welded portion relative to the folded-back bent portion to come into contact with at least one bending roller in the roller pair group to form the front end side bent portion.
[0029] According to the present disclosure, a laminated battery having a weld portion having excellent impact resistance against external impact and a method for manufacturing the laminated battery can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a schematic cross-sectional view illustrating a laminated battery according to this embodiment.
[0031] Figure 2 This is a schematic cross-sectional view of a laminated battery illustrating another form of the present embodiment.
[0032] Figure 3 This is a schematic cross-sectional view of a laminated battery illustrating another form of the present embodiment.
[0033] Figure 4 This is a schematic cross-sectional view of a laminated battery illustrating another form of the present embodiment.
[0034] Figure 5 This is a schematic cross-sectional view showing an example of a solid state battery.
[0035] Description of Reference Numerals
[0036] 2 Electrode body
[0037] 4 Laminated film
[0038] 10A, 10B, 10C laminated batteries
[0039] 20 End face
[0040] 40a, 42a, 42b, 42d, 44a Right angle bend
[0041] 40b, 42c, 44b: folded back bends
[0042] 40c, 42e, 44c: distal end side bending portion
[0043] 400, 420, 440 Top
[0044] 101 Negative electrode active material
[0045] 103 Coated positive electrode active material
[0046] 105, 107 Conductive additives
[0047] 109, 111 Adhesives
[0048] 113 negative electrode collector
[0049] 115 positive electrode collector
[0050] A Negative electrode active material layer
[0051] B Solid electrolyte layer
[0052] C Positive electrode active material layer DETAILED DESCRIPTION
[0053] <Laminated battery>
[0054] The laminated battery of the embodiment of the present disclosure comprises: an electrode body, and a laminate film covering the electrode body and sealing it inside, the laminate film having a weld portion in which the ends overlap each other to weld the inner surfaces, the weld portion having three or more bends, the three or more bends comprising: two or more bends bent at an angle of less than 90° into an angle or an arc, and one top side bend bent at an angle of less than 180° at the topmost position of the weld portion into an angle or an arc, the weld portion having a shape in which at least a portion of the top end is directed toward the electrode body side.
[0055] Since at least a portion of the top of the weld is directed toward the electrode body, even when an impact is applied to the weld from the outside, the top will first contact the electrode body (the laminate film covering the electrode body) and be blocked, and then even when an impact is applied to the weld from the outside, the weld will be difficult to deform. As a result, the impact resistance of the weld is improved, and as a result, the damage of the electrode body can be suppressed.
[0056] Hereinafter, one embodiment of the laminated battery of the present disclosure will be described with reference to the drawings.
[0057] Each of the following drawings is a schematic diagram, and the size and shape of each part are appropriately exaggerated for easy understanding.
[0058] (First method)
[0059] Figure 1This is a schematic cross-sectional view illustrating a laminated battery according to this embodiment.
[0060] The laminated battery 10A includes an electrode body 2 and a laminate film 4 covering and sealing the electrode body 2. The laminate film 4 has a welded portion 40 where one end side and the other end side overlap and the inner surfaces are welded to each other. The electrode body 2 has an end face 20 ( Figure 1 The end face of the welding portion 40 is formed into an inclined surface. The welding portion 40 is formed in the end face 20 of the electrode body 2 as an inclined surface, and the end portion ( Figure 1 The welding portion 40 is formed toward the outside from the root side of the welding portion 40 (that is, the position closest to the electrode body 2) to the top 400 side, and has a total of three bends, which are a right-angled bend 40a bent into an arc at an angle of approximately 90°, a folded-back bend 40b bent into an arc at an angle of approximately 0°, and a top-side bend 40c bent into an arc at an angle of approximately 90° at the position closest to the top 400 of the welding portion 40. The top-side bend 40c is arranged at a position closest to the right-angled bend 40a of the bend closest to the root side of the welding portion 40, among all the remaining bends (that is, the right-angled bend 40a and the folded-back bend 40b).
[0061] Here, the angle of the welded portion in the present disclosure refers to the minimum angle formed by the welded portions on both sides sandwiching the bent portion.
[0062] The weld portion 40 has a shape in which the tip 400 faces the electrode body 2 side. Figure 1 The welded portion 40 shown is in the longitudinal direction of the welded portion 40 ( Figure 1 The shape has a top 400 in which all regions thereof (in the depth direction) are oriented toward the electrode body 2 side.
[0063] Here, “having a shape with the tip facing the electrode body side” means that the tip of the weld portion is arranged closer to the electrode body than the tip-side bent portion.
[0064] so, Figure 1 The laminated battery 10A shown has a shape in which the top end 400 faces the electrode body 2. Assume that an impact is applied to the welded portion 40 from the outside, for example, Figure 1 In this case, the weld 40 is deformed starting from the right-angled bend 40a, and the top 400 is initially blocked by the electrode body 2 side (the laminate film 4 covering the electrode body 2). Then, even if further impact is applied from the outside (for example, from Figure 1Since the welding portion 40 is continuously impacted (in the right direction in FIG. 1 ), the tip portion 400 is also in contact with the electrode body 2 side, so that the welding portion 40 is difficult to deform. As a result, the impact resistance of the welding portion 40 is improved, and as a result, the electrode body 2 can be prevented from being damaged due to the impact applied to the welding portion 40.
[0065] Furthermore, Figure 1 Although the embodiment shows a configuration having three curved portions curved in an arc shape, the curved portions may be curved in an angular shape, that is, in a shape having an angle.
[0066] In addition, Figure 1 , the entire region of the top 400 in the longitudinal direction of the weld 40 has a shape facing the electrode body 2 side, but it is sufficient as long as the top of the weld has at least a portion facing the electrode body side. By making at least a portion of the top of the weld face the electrode body side, even if an impact is applied to the weld from the outside, the top of a portion facing the electrode body side will first contact the electrode body side and be blocked, so that the impact resistance of the weld is improved, and damage to the electrode body can be suppressed.
[0067] Furthermore, the laminated battery of the embodiment of the present disclosure only needs to have three or more bends, and the three or more bends include: two or more bends bent at an angle of less than 90° in the weld to form a rectangle or arc; and one top bend bent at an angle of less than 180° at the topmost position of the weld to form an angle or arc. The weld has as a bend: one or more right-angle bends bent at an angle of more than 70° and less than 90° to form an angle or arc, and one folded-back bend bent at an angle of less than 20° to form an angle or arc, which is preferred from the viewpoint of improving the structural efficiency of the weld.
[0068] (Second method)
[0069] Figure 2 This is a schematic cross-sectional view of a laminated battery illustrating another form of the present embodiment.
[0070] The laminated battery 10B has an electrode body 2 and a laminate film 4 covering the electrode body 2 and sealing it inside. The laminate film 4 has a weld 42 in which one end side and the other end side overlap and the inner surfaces are welded to each other. The weld 42 has a total of 5 bends from the root side of the weld 42 (that is, the position closest to the electrode body 2) to the top 420 side. The total of 5 bends are a right-angle bend 42a bent into an arc at an angle of approximately 90°, a right-angle bend 42b bent into an arc at an angle of approximately 90°, a folded-back bend 42c bent into an arc at an angle of approximately 0°, a right-angle bend 42d bent into an arc at an angle of approximately 90°, and a top side bend 42e bent into an arc at an angle of approximately 90° at the position closest to the top 420 of the weld 42. The distal end side bend 42e is arranged at a position closest to the right-angle bend 42a corresponding to the bend on the most root side of the weld 42 among all the remaining bends (ie, the right-angle bends 42a, 42b, 42d and the folded bend 42c).
[0071] The weld portion 42 has a shape in which the tip 420 faces the electrode body 2. That is, the tip 420 of the weld portion 42 is disposed closer to the electrode body 2 than the tip-side bent portion 42e. Figure 2 The welded portion 42 shown is in the longitudinal direction of the welded portion 42 ( Figure 2 The shape has a top 420 in which all regions thereof (in the depth direction) are oriented toward the electrode body 2 side.
[0072] so, Figure 2 The laminated battery 10B shown has a shape in which the top end 420 faces the electrode body 2. Assume that an impact is applied to the welded portion 42 from the outside, for example, Figure 2 In this case, the weld 42 is deformed starting from the right-angled bend 42a, and the folded bend 42c first contacts the electrode body 2 side (the laminate film 4 covering the electrode body 2). However, it is considered that by further continuous application of the impact, the folded bend 42c in contact with the electrode body 2 side slips (towards the right side). Figure 2 Then, if the impact is further applied to the welded portion 42, the top portion 420 contacts the electrode body 2 side (the laminate film 4 covering the electrode body 2) and is blocked. Then, even if the impact is further applied from the outside (for example, from Figure 2 The welding portion 42 is continuously impacted by the top end 420 and the electrode body 2, and the welding portion 42 is not easily deformed because the top end 420 is in contact with the electrode body 2. As a result, the impact resistance of the welding portion 42 is improved, and as a result, the electrode body 2 can be prevented from being damaged by the impact applied to the welding portion 42.
[0073] Furthermore, Figure 2Although the embodiment shows an embodiment having five curved portions curved in an arc shape, the curved portions may be curved in an angular shape, that is, in a shape having an angle.
[0074] in addition, Figure 2 2 shows an embodiment in which the entire region of the tip 420 of the weld 42 in the longitudinal direction thereof faces the electrode body 2 , but the tip of the weld 420 only needs to have a shape in which at least a portion of the tip faces the electrode body 2 .
[0075] (Third method)
[0076] Figure 3 This is a schematic cross-sectional view showing another form of a laminated battery according to the present embodiment.
[0077] The laminated battery 10C has an electrode body 2 and a laminate film 4 covering the electrode body 2 and sealing it inside. The laminate film 4 has a welded portion 44 in which one end side and the other end side overlap and the inner surfaces are welded to each other. The welded portion 44 has a total of three bends from the root side of the welded portion 44 (that is, the position closest to the electrode body 2) to the top end 440 side. The total of three bends are a right-angle bend 44a bent into an arc at an angle of approximately 90°, a folded bend 44b bent into an arc at an angle of approximately 0°, and a top end side bend 44c bent into an arc at an angle of approximately 90° at the position closest to the top end 440 of the welded portion 44.
[0078] The distal end side bent portion 44c is arranged at a position closest to the turned-back bent portion 44b which is not a bent portion on the most root side of the fusion portion 44 among all the remaining bent portions (ie, the right-angled bent portion 44a and the turned-back bent portion 44b).
[0079] The weld portion 44 has a shape in which the tip 440 faces the electrode body 2. That is, the tip 440 of the weld portion 44 is disposed closer to the electrode body 2 than the tip-side bent portion 44c. Figure 3 The welded portion 44 shown is in the longitudinal direction of the welded portion 44 ( Figure 3 The shape has a top 440 in which all regions thereof (in the depth direction) are oriented toward the electrode body 2 side.
[0080] so, Figure 3 The laminated battery 10C shown has a shape in which the top end 440 faces the electrode body 2. Assume that an impact is applied to the welded portion 44 from the outside, for example, Figure 3 In the case where an impact is applied to the weld 44 from the right side of the welding line. At this time, the weld 44 is deformed starting from the right-angle bend 44a, and the top end 440 first contacts the electrode body 2 side (the laminate film 4 covering the electrode body 2) and is blocked. Then, even if further impact is applied from the outside (for example, from Figure 3The welding portion 44 is continuously impacted (in the right direction in FIG. 1 ), and since the tip portion 440 is in contact with the electrode body 2 side, the welding portion 44 is also difficult to deform. As a result, the impact resistance of the welding portion 44 is improved, and as a result, the electrode body 2 can be prevented from being damaged due to the impact applied to the welding portion 44.
[0081] Furthermore, Figure 3 Although the embodiment shows an embodiment having three curved portions curved in an arc shape, the curved portions may be curved in an angular shape, that is, in a shape having an angle.
[0082] In addition, Figure 3 In the figure, the entire region of the tip 440 of the weld 44 in the longitudinal direction is oriented toward the electrode body 2 , but the weld may be shaped such that at least a portion of the tip 440 is oriented toward the electrode body 2 .
[0083] exist Figure 1 to Figure 3 In the first to third embodiments shown, the end surface of the electrode body is an inclined surface, but the shape of the electrode body is not limited to this. Figure 4 As shown, a rectangular parallelepiped electrode body 2D may also be used.
[0084] In the laminated battery of the embodiment of the present disclosure, the top of the weld has a shape facing the electrode body. From the viewpoint of improving the impact resistance of the weld to external impact, the shortest distance between the top of the weld and the laminate film covering the electrode body is preferably 0.5 mm to 5 mm, more preferably 0.5 mm to 1 mm. Furthermore, the shortest distance between the top of the weld and the laminate film covering the electrode body is, for example, Figure 1 The distance a1 is in Figure 2 The distance a2 is in the middle. Figure 3 The middle refers to the distance a3, Figure 4 The middle refers to the distance a4.
[0085] exist Figure 1 to Figure 3 In the first to third embodiments shown, a laminated battery is shown in which an electrode body is covered with a single laminate film. However, the present disclosure is not limited thereto, and a laminated battery may be used in which an electrode body is covered with a plurality of laminate films. For example, a laminated battery may be used in which an electrode body is covered with two laminate films, and the ends of the two laminate films are overlapped and their inner surfaces are welded to form a welded portion to seal the electrode body.
[0086] <Method for manufacturing laminated battery>
[0087] Next, a method for manufacturing a laminated battery according to an embodiment of the present disclosure will be described.
[0088] A method for manufacturing a laminated battery In a method for manufacturing the following laminated battery, the laminated battery has an electrode body and a laminate film covering the electrode body and sealing it inside, the laminate film has a weld portion with ends overlapping each other and inner surfaces welded together, the weld portion has more than three bends, and the more than three bends include: more than two bends bent at an angle of less than 90° into an angle or arc shape, and one top side bend bent at an angle of less than 180° at the topmost position of the weld portion into an angle or arc shape, the weld portion has a shape with at least a portion of the top end facing the electrode body side, the weld portion has as a bend portion one folded back bend bent at an angle of less than 20° into an angle or arc shape, and one or more right-angle bends formed on the root side of the weld portion closer to the folded back bend and bent at an angle of more than 70° and less than 90° into an angle or arc shape.
[0089] Furthermore, the method for manufacturing a laminated battery has:
[0090] A step of preparing a welded laminated battery having a planar welded portion formed by overlapping the ends of the laminated films and welding the inner surfaces thereof;
[0091] A folding and bending step of forming a folded and bent portion bent at an angle of 20° or less in an angular or arc shape at the fusion-bonded portion of the laminated battery after fusion bonding; and
[0092] The right-angle bending step is to form a right-angled bent portion bent into an angle or arc shape at an angle of 70° or more and 90° or less in a region closer to the root side of the weld portion than the folded-back bent portion.
[0093] The right-angle bending step is a step of bending the welded portion in stages to form a right-angle bent portion by conveying between each pair of rollers in a roller pair group, wherein the roller pair group includes: at least three bending rollers in contact with the surface of the bending side of the welded portion and having different contact angles with respect to the welded portion, and opposing rollers provided at positions opposing the bending rollers across the welded portion and having the same number as the bending rollers;
[0094] Furthermore, the right-angle bending step is a step of bringing a region on the front end side of the fusion portion relative to the folded-back bent portion into contact with at least one bending roller in the roller pair group to form a front end side bent portion.
[0095] · Example of manufacturing the laminated battery of the first embodiment
[0096] First, Figure 1 The right-angled bend 40a, the folded bend 40b and the front end bend 40c in the first embodiment of the laminated battery 10A can be formed by performing the folding and right-angled bending steps described below.
[0097] First, a laminated battery having an unbent planar welded portion 40 (laminated battery after welding) is subjected to a bending operation to form a folded-back bent portion 40b (folding-back bending process). The bending operation in the folding-back bending process may be performed by, for example, the following method: the welded portion 40 is bent in stages by conveying it between each pair of rollers in a roller pair group, the roller pair group having: a plurality of bending rollers in contact with the surface of the folded side of the welded portion 40 (that is, the valley folded side of the folded-back bent portion 40b) and having different contact angles with respect to the welded portion 40, and opposing rollers provided at positions opposing the bending rollers across the welded portion 40 and having the same number as the bending rollers.
[0098] Next, the weld 40 formed with the folded-back bent portion 40b is bent in a region closer to the root side of the weld 40 than the folded-back bent portion 40b to form a right-angle bent portion 40a (right-angle bending step). The bending operation in the right-angle bending step can be, for example, the following method: the weld 40 is bent in stages by conveying it between each pair of rollers in a roller pair group, the roller pair group having: three bending rollers in contact with the surface of the bending side of the weld 40 (that is, the valley fold side of the right-angle bent portion 40b) and having different contact angles with respect to the weld 40, and opposing rollers provided at positions opposing the bending rollers across the weld 40 and having the same number as the bending rollers.
[0099] Furthermore, in the right-angle bending step, by bringing the region closer to the tip 400 side of the weld 40 than the folded-back bent portion 40b into contact with at least one bending roller in the roller pair group, the tip side bent portion 40c can be further formed. Furthermore, when bringing at least one bending roller in the roller pair group into contact with the region on the tip 400 side of the weld 40, the entire region of the tip 400 in the longitudinal direction of the weld 40 may be brought into contact, or only a portion of the tip 400 of the weld 40 may be brought into contact.
[0100] In the right-angle bending step, the right-angle bent portion 40a is formed by using the above-mentioned roller pair group having at least three bending rollers with different contact angles, and the tip-side bent portion 40c is formed by making at least one bending roller in the above-mentioned roller pair group contact the region on the tip 400 side of the weld 40, thereby suppressing the occurrence of springback in the weld 40. In addition, at least a portion of the tip 400 of the weld 40 can be shaped to face the electrode body 2 side, thereby improving the impact resistance of the weld 40.
[0101] · Example of manufacturing the laminated battery of the second embodiment
[0102] As Figure 2The second embodiment of the laminated battery manufacturing method can be a method in which, in the above-mentioned first embodiment of the laminated battery manufacturing example, a second right-angle bending step is further performed after the folding back bending step and before the right-angle bending step, or after the right-angle bending step.
[0103] That is, the folded-back bent portion 42c is formed in the same manner as in the manufacturing example of the laminated battery of the first embodiment (folded-back bending process), and then the right-angled bent portion 42a and the top-side bent portion 42e are formed in the same manner as in the manufacturing example of the laminated battery of the first embodiment (right-angled bending process). Then, right-angled bent portions 42b and 42d are formed in the region between the folded-back bent portion 42c and the top-side bent portion 42e, and in the region between the folded-back bent portion 42c and the right-angled bent portion 42a, respectively (second right-angled bending process). The bending operation in the second right-angle bending step can be, for example, a method in which the welded portion 42 is bent in stages by conveying it between each pair of rollers in a roller pair group, the roller pair group including a plurality of bending rollers that are in surface contact with the bending side of the welded portion 42 (that is, the valley fold side of the right-angle bent portion 42d) and have different contact angles with respect to the welded portion 42, and opposing rollers that are provided at positions opposing the bending rollers across the welded portion 42 and have the same number as the bending rollers. Furthermore, the second right-angle bending step may be performed after the folding back bending step and before the right-angle bending step.
[0104] According to the second embodiment of the laminated battery manufacturing example described above, springback can be suppressed at weld 42. Also, at least a portion of top 420 of weld 42 can be shaped to face electrode body 2, thereby improving the impact resistance of weld 42.
[0105] Furthermore, the method for manufacturing the laminated battery according to the embodiment of the present disclosure is not limited to the above method. Figure 3 The method for manufacturing the laminated battery of the third embodiment shown may include a method in which the right-angled bent portion 44 a , the folded-back bent portion 44 b , and the distal end bent portion 44 c are formed by separate bending steps.
[0106] (Battery components)
[0107] Next, the electrode body and the laminate film constituting the laminated battery of the present embodiment will be described.
[0108] (1) Laminated film
[0109] As the laminated film, for example, there can be mentioned a film having a metal layer, and there can also be mentioned a three-layer structure film having resin layers on both sides of the metal layer. Furthermore, in the three-layer structure film, the resin layer on the inner side to be the electrode body side (that is, the fused resin layer) is used as the fusion resin layer, and the resin layer on the outer peripheral side opposite to the electrode body side is used as the protective resin layer.
[0110] Examples of materials for the welding resin layer include olefin resins such as polypropylene (PP) and polyethylene (PE). Examples of materials for the metal layer include aluminum, aluminum alloys, and stainless steel. Examples of materials for the protective resin layer include polyethylene terephthalate (PET) and nylon. The thickness of the welding resin layer is, for example, greater than 40 μm and less than 100 μm. The thickness of the metal layer is, for example, greater than 30 μm and less than 60 μm. The thickness of the protective resin layer is, for example, greater than 20 μm and less than 60 μm. The thickness of the entire laminate film is, for example, greater than 70 μm and less than 220 μm.
[0111] (2) Electrode body
[0112] The electrode body functions as a power generation element of the battery. The shape of the electrode body is not particularly limited, and examples thereof include a rectangular parallelepiped shape, a shape with an inclined end face, etc. The electrode body usually has a positive electrode collector, a positive electrode active material layer, an electrolyte layer, a negative electrode active material layer, and a negative electrode collector in order in the thickness direction.
[0113] The positive electrode active material layer contains at least a positive electrode active material. The positive electrode active material layer may further contain at least one of a conductive material, an electrolyte, and a binder. The shape of the positive electrode active material is, for example, granular. As the positive electrode active material, for example, an oxide active material can be cited. In addition, sulfur (S) can also be used as the positive electrode active material.
[0114] As the positive electrode active material, it is preferred to contain a lithium composite oxide. The lithium composite oxide may also contain at least one selected from F, Cl, N, S, Br and I. In addition, the lithium composite oxide may also have a crystal structure belonging to at least one space group selected from space groups R-3m, Immm and P63-mmc (also referred to as P63mc, P6 / mmc). In addition, the main arrangement of transition metals, oxygen and lithium in the lithium composite oxide may also be an O2 type structure.
[0115] Examples of lithium composite oxides having a crystal structure belonging to R-3m include Li x Me y O α X β (Me represents at least one selected from Mn, Co, Ni, Fe, Al, Cu, V, Nb, Mo, Ti, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, W, B, Si and P, X represents at least one selected from F, Cl, N, S, Br and I, and satisfies 0.5≤x≤1.5, 0.5≤y≤1.0, 1≤α<2 and 0<β≤1).
[0116] As a lithium composite oxide having a crystal structure belonging to Immm, for example, a composite oxide represented by Li x1 M 1 A 1 2 (satisfying 1.5 ≤ x1 ≤ 2.3, M 1 contains at least one selected from Ni, Co, Mn, Cu, and Fe, A 1 contains at least oxygen, and the ratio of oxygen in A 1 is 85 atomic% or more) (a specific example is Li2NiO2), a composite oxide represented by Li x1 M 1A 1-x2 M 1B x2 O 2-y A 2 y (0 ≤ x2 ≤ 0.5, 0 ≤ y ≤ 0.3, at least one of x2 and y is not 0, M 1A represents at least one selected from Ni, Co, Mn, Cu, and Fe, M 1B represents at least one selected from Al, Mg, Sc, Ti, Cr, V, Zn, Ga, Zr, Mo, Nb, Ta, and W, and A2 represents at least one selected from F, Cl, Br, S, and P).
[0117] As a lithium composite oxide having a crystal structure belonging to P63 - mmc, for example, a composite oxide represented by M1 x M2 y O2 (M1 represents an alkali metal (preferably at least one of Na and K), M2 represents a transition metal (preferably at least one selected from Mn, Ni, Co, and Fe), and x + y satisfies 0 < x + y ≤ 2).
[0118] As a lithium composite oxide having an O2 - type structure, for example, a composite oxide represented by Li x [Li α (Mn a Co b M c ) 1-α O2 (0.5 < x < 1.1, 0.1 < α < 0.33, 0.17 < a < 0.93, 0.03 < b < 0.50, and 0.04 < c < 0.33, M represents at least one selected from Ni, Mg, Ti, Fe, Sn, Zr, Nb, Mo, W, and Bi), and as a specific example, Li 0.744 [Li 0.145 Mn 0.625 Co 0.115 Ni 0.115 O2 etc. can be cited.
[0119] In addition, the positive electrode preferably contains, in addition to the positive electrode active material, a solid electrolyte selected from the group of solid electrolytes consisting of sulfide solid electrolytes, oxide solid electrolytes, and halide solid electrolytes, and more preferably, at least a part of the surface of the positive electrode active material is coated with a sulfide solid electrolyte, an oxide solid electrolyte, or a halide solid electrolyte. As the halide solid electrolyte coating at least a part of the surface of the positive electrode active material, Li 6-(4-x)b (Ti 1-x Al x ) b F6 (0 < x < 1, 0 < b ≤ 1.5) [LTAF electrolyte].
[0120] Examples of the conductive material include carbon materials. The electrolyte can be a solid electrolyte or a liquid electrolyte. The solid electrolyte can be an organic solid electrolyte such as a gel electrolyte, or an inorganic solid electrolyte such as an oxide solid electrolyte or a sulfide solid electrolyte. In addition, the liquid electrolyte (electrolyte solution) contains, for example, a supporting salt such as LiPF6 and a solvent such as a carbonate-based solvent. In addition, examples of the binder include a rubber-based binder and a fluoride-based binder.
[0121] The negative electrode active material layer contains at least a negative electrode active material. The negative electrode active material layer may further contain at least one of a conductive material, an electrolyte, and a binder. Examples of the negative electrode active material include metal active materials such as Li and Si, carbon active materials such as graphite, and oxide active materials such as Li4Ti5O 12 and the like. The shape of the negative electrode current collector is, for example, foil-shaped or net-shaped. Regarding the conductive material, the electrolyte, and the binder, they are the same as the above content.
[0122] The electrolyte layer is disposed between the positive electrode active material layer and the negative electrode active material layer and contains at least an electrolyte. The electrolyte can be a solid electrolyte or a liquid electrolyte. As the electrolyte layer, a solid electrolyte layer is preferred. The electrolyte layer may also have a separator.
[0123] As the solid electrolyte, it is preferred to contain at least one solid electrolyte selected from the group of solid electrolytes consisting of sulfide solid electrolytes, oxide solid electrolytes, and halide solid electrolytes.
[0124] As a sulfide solid electrolyte, it preferably contains sulfur (S) as the main component of the anion element, and more preferably contains, for example, Li element, A element and S element. The A element is at least one selected from P, As, Sb, Si, Ge, Sn, B, Al, Ga and In. The sulfide solid electrolyte may also contain at least one of O and halogen elements. As the halogen element (X), for example, F, Cl, Br, I, etc. can be cited. The composition of the sulfide solid electrolyte is not particularly limited, and examples thereof include xLi2S·(100-x)P2S5 (70≤x≤80), yLiI·zLiBr·(100-y-z)(xLi2S·(1-x)P2S5) (0.7≤x≤0.8, 0≤y≤30, 0≤z≤30). The sulfide solid electrolyte may also have a composition represented by the following general formula (1).
[0125] Li 4-x Ge 1-x P x S4 (0<x<1) Formula (1)
[0126] In the formula (1), at least a part of Ge may also be substituted by at least one selected from Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V and Nb. In addition, at least a part of P may also be substituted by at least one selected from Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V and Nb. A part of Li may also be substituted by at least one selected from Na, K, Mg, Ca and Zn. A part of S may also be substituted by a halogen. As the halogen, it is at least one of F, Cl, Br and I.
[0127] As an oxide solid electrolyte, it preferably contains oxygen (O) as the main component of the anion element, and for example, it may also contain Li, Q element (Q represents at least one of Nb, B, Al, Si, P, Ti, Zr, Mo, W and S) and O. As the oxide solid electrolyte, garnet-type solid electrolyte, perovskite-type solid electrolyte, NASICON-type solid electrolyte, Li-P-O-based solid electrolyte, Li-B-O-based solid electrolyte, etc. can be cited. As the garnet-type solid electrolyte, for example, Li7La3Zr2O 12 、Li 7-x La3(Zr 2-x Nb x )O 12 (0≤x≤2), Li5La3Nb2O 12etc. As perovskite-type solid electrolytes, examples include (Li, La)TiO3, (Li, La)NbO3, (Li, Sr)(Ta, Zr)O3, etc. As NASICON-type solid electrolytes, examples include Li(Al, Ti)(PO4)3, Li(Al, Ga)(PO4)3, etc. As Li-P-O-based solid electrolytes, Li3PO4 and LIPON (a compound in which part of the O in Li3PO4 is replaced by N) can be mentioned. As Li-B-O-based solid electrolytes, Li3BO3 and a compound in which part of the O in Li3BO3 is replaced by C, etc., can be mentioned.
[0128] As the halide solid electrolyte, it is suitable to use a solid electrolyte containing Li, M, and X (M represents at least one of Ti, Al, and Y, and X represents F, Cl, or Br). Specifically, Li 6-3z Y z X6 (X represents Cl or Br, and z satisfies 0 < z < 2), Li 6-(4-x)b (Ti 1-x Al x ) b F6 (0 < x < 1, 0 < b ≤ 1.5). In Li 6-3z Y z X6, considering the excellent lithium ion conductivity, Li3YX6 (X represents Cl or Br) is more preferred, and Li3YCl6 is further preferred. In addition, Li 6-(4-x)b (Ti 1-x Al x ) b F6 (0 < x < 1, 0 < b ≤ 1.5) is preferably contained together with a solid electrolyte such as a sulfide solid electrolyte, for example, from the viewpoint of suppressing the oxidative decomposition of the sulfide solid electrolyte.
[0129] The positive electrode current collector collects the current of the positive electrode active material layer. Examples of the positive electrode current collector include stainless steel, aluminum, nickel, iron, titanium, carbon, etc., and aluminum alloy foil or aluminum foil is preferred. The aluminum alloy foil and the aluminum foil can also be manufactured using powder. The shape of the positive electrode current collector is, for example, foil-shaped or mesh-shaped.
[0130] The negative electrode current collector collects the current of the negative electrode active material layer. As the material of the negative electrode current collector, examples of metals include copper, SUS, nickel, etc. As the shape of the negative electrode current collector, examples include foil-shaped or mesh-shaped.
[0131] · Battery structure
[0132] The structure of a solid battery has a stacked structure of positive electrode / solid electrolyte layer / negative electrode. Solid batteries include so-called all-solid batteries that use solid electrolytes as electrolytes. The solid electrolyte may also contain an electrolyte solution that is less than 10% by mass relative to the total amount of the electrolyte. Furthermore, the solid electrolyte may also be a composite solid electrolyte containing an inorganic solid electrolyte and a polymer electrolyte.
[0133] The positive electrode has a positive electrode active material layer and a current collector, and the negative electrode has a negative electrode active material layer and a current collector.
[0134] The solid electrolyte layer may have a single-layer structure or a multi-layer structure of two or more layers.
[0135] Solid state batteries may have, for example, Figure 5 The cross-sectional structure shown in FIG. 1 may also be a solid electrolyte layer B. Figure 5 The double-layer structure shown. Figure 5 This is a schematic cross-sectional view showing an example of a solid state battery. Figure 5 The solid battery shown has a negative electrode including a negative electrode collector 113 and a negative electrode active material layer A, a solid electrolyte layer B, and a positive electrode including a positive electrode collector 115 and a positive electrode active material layer C. The negative electrode active material layer A includes a negative electrode active material 101, a conductive auxiliary agent 105, and a binder 109. The positive electrode active material layer C includes a coated positive electrode active material 103, a conductive auxiliary agent 107, and a binder 111, and the surface of the positive electrode active material of the coated positive electrode active material 103 is coated with an LTAF electrolyte or a LiNbO3 electrolyte.
[0136] In addition, a solid battery can also be formed by sealing the stacked end faces (side faces) of the stacked structure of the positive electrode / solid electrolyte layer / negative electrode with a resin. The current collector of the electrode can also be a structure with a buffer layer, an elastic layer or a PTC (Positive Temperature Coefficient) thermistor layer arranged on the surface.
[0137] ·Battery
[0138] Typically, the laminated battery in the present disclosure is a lithium ion secondary battery. As the purpose of the battery, for example, a power source for a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), an electric vehicle (BEV), a gasoline vehicle, a diesel vehicle, etc. can be cited. It is particularly preferably used as a driving power source for a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV) or an electric vehicle (BEV). In addition, the battery in the present disclosure can be used as a power source for a mobile body (e.g., a railway, a ship, an airplane) other than a vehicle, and can also be used as a power source for electrical products such as an information processing device.
[0139] The present disclosure is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative, and all schemes having substantially the same technical ideas as those described in the scope of the claims in the present disclosure and having the same functions and effects are included in the technical scope of the present disclosure.
Claims
1. A laminated battery having: Electrode body, and a laminate film covering the electrode body and sealing it inside, The laminate film has a welded portion where the ends overlap each other and the inner surfaces are welded together, The welded portion has three or more bends, and the three or more bends include: Two or more bent portions bent at an angle of 90° or less into an angle or an arc, and a top end side bent portion bent at an angle of less than 180° into an angle or an arc at the most top end position of the weld portion, The weld portion has a shape in which at least a portion of a tip thereof faces the electrode body.
2. The laminated battery according to claim 1, The bending portion and the top end side bending portion are both bent into an arc shape.
3. The laminated battery according to claim 1, The position where the distal end side bent portion is arranged is a position closest to the bent portion closest to the root side of the fusion portion among the two or more bent portions.
4. The laminated battery according to claim 1, The shortest distance between the tip of the weld and the laminate film covering the region of the electrode body is 0.5 mm to 5 mm.
5. The laminated battery according to claim 1, The weld portion has as the bent portion: one folded-back bent portion bent at an angle of 20° or less into an angular or arc shape, and one or more right-angled bent portions formed on the root side of the weld portion relative to the folded-back bent portion and bent at an angle of 70° or more and 90° or less into an angular or arc shape.
6. A method for manufacturing a laminated battery according to claim 5, comprising: A step of preparing a welded laminated battery having a planar welded portion formed by overlapping the ends of the laminated films and welding the inner surfaces thereof; A folding and bending step, wherein the fused portion in the fused laminated battery is formed into a folded and bent portion bent at an angle of 20° or less into an angular or arc shape; as well as The right-angle bending step is to form a right-angled bent portion bent into an angle or an arc shape at an angle of 70° or more and 90° or less in a region closer to the root side of the weld portion than the folded-back bent portion. The right-angle bending step is a step of bending the welded portion in stages to form the right-angle bent portion by conveying between each pair of rollers in a roller pair group, wherein the roller pair group comprises: at least three bending rollers in contact with the surface of the bending side of the welded portion and having different contact angles with respect to the welded portion, and opposing rollers provided at positions opposing the bending rollers across the welded portion and having the same number as the bending rollers; Furthermore, the right-angle bending step is a step of causing a region on the front end side of the welded portion relative to the folded-back bent portion to come into contact with at least one bending roller in the roller pair group to form the front end side bent portion.
Citation Information
Patent Citations
Manufacturing method for secondary battery
JP2019200973A