Three-electrode soft package battery and preparation method thereof

By using reference electrodes coated with lithium iron phosphate on both sides and charging and discharge activation treatment in a three-electrode soft-pack battery, the complex problem of dissolution and preparation of reference electrodes at high temperatures is solved, and the stability and monitoring accuracy of the battery are achieved , simplifies the battery preparation process.

CN119069771AActive Publication Date: 2024-12-03SHENZHEN BAK POWER BATTERY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411086254.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-12-03
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing three-electrode lithium-ion batteries are very easy to dissolve in the reference electrode copper wire plated at high temperatures, resulting in inaccurate test data and are not suitable for the positive and negative voltage monitoring of long-circulating batteries. Moreover, the preparation of lithium iron phosphate reference electrodes is complicated. And fragile and difficult to scale.

Method used

A three-electrode soft-pack battery structure is adopted, in which the reference electrode is coated with lithium iron phosphate on both sides, with a small and stable area, located in the positive middle of the positive electrode sheet and the negative electrode sheet, and the battery is activated to a state of charge by charging and discharging cycle. , ensure the stability of the reference electrode and the uniformity of the battery.

Benefits of technology

The stability of the reference electrode and the uniformity of the battery are achieved, and are suitable for the monitoring of positive and negative electrode voltages during long cycles, simplifying the battery preparation process, reducing the production complexity and material loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069771A_ABST
    Figure CN119069771A_ABST
Patent Text Reader

Abstract

The invention discloses a three-electrode soft package battery and a preparation method thereof. The three-electrode soft package battery comprises a soft package shell, an electrolyte, a diaphragm, a positive plate, a negative plate and a reference electrode, the electrolyte is sealed in the soft package shell, and the positive plate, the diaphragm, the reference electrode, the diaphragm and the negative plate are sequentially stacked and immersed in the electrolyte; the positive plate, the negative plate and the reference electrode are correspondingly connected with a positive tab, a negative tab and a reference electrode tab which are positioned outside the soft package shell respectively; wherein the surface of the reference electrode is coated with lithium iron phosphate, and the area ratio of the reference electrode to the positive plate is 0.001-0.01. The three-electrode soft package battery disclosed by the invention is simple in structure and easy to prepare quickly; the influence of the reference electrode on the total battery capacity is small; the reference electrode is stable, and is suitable for real-time monitoring of positive and negative electrode voltages in a long cycle process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a three-electrode soft-pack battery and a preparation method thereof. Background Art

[0002] With the popularity of new energy vehicles, the performance requirements for lithium-ion batteries are getting higher and higher, and the update and iteration speed of lithium-ion power batteries is getting faster and faster. Therefore, it is particularly important to improve the efficiency of the system evaluation of power batteries. Among the system evaluation methods and evaluation means of lithium-ion power batteries, soft-pack laminated batteries are particularly suitable for early system evaluation because they are simple to prepare and can basically simulate the actual performance of the full battery system, which is conducive to shortening the test evaluation cycle and improving test efficiency.

[0003] In recent years, the use of three-electrode batteries to study the potential changes, impedance changes, lithium plating behavior, etc. of lithium-ion batteries under different conditions has become an important evaluation method.

[0004] Among the reference electrodes widely used at present, the copper wire reference electrode has the advantages of simple and low cost in preparation. However, in actual use, the metallic lithium plated on the copper wire of the reference electrode is extremely active and will dissolve in the battery system in a short time at high temperature, affecting the judgment of the battery data in the test. At the same time, the copper wire needs to be re-plated with lithium, which is not suitable for monitoring the positive and negative electrode voltages of long-cycle batteries. Lithium iron phosphate can be used as a stable reference electrode due to its relatively stable lithium deintercalation voltage platform, especially for monitoring the positive and negative electrode voltages of batteries in long cycles. Summary of the invention

[0005] The purpose of this application is to provide a three-electrode soft-pack battery and a preparation method thereof.

[0006] In order to solve the above problems, this application adopts the following technical solutions:

[0007] The first aspect of the present application discloses a three-electrode soft-pack battery, characterized in that it includes: a soft-pack shell, an electrolyte, a diaphragm, a positive electrode sheet, a negative electrode sheet and a reference electrode; the electrolyte is sealed in the soft-pack shell, the positive electrode sheet, the diaphragm, the reference electrode, the diaphragm and the negative electrode sheet are stacked in sequence and immersed in the electrolyte; the positive electrode sheet, the negative electrode sheet and the reference electrode are respectively connected to the positive electrode tab, the negative electrode tab and the reference electrode tab located outside the soft-pack shell; wherein the reference electrode is coated with lithium iron phosphate on both sides, and the area ratio of the reference electrode to the positive electrode sheet is 0.001 to 0.01. It should be noted that the three-electrode soft-pack battery of the present application has a simple structure, and the reference electrode contains lithium iron phosphate. Lithium iron phosphate has a relatively stable lithium deintercalation voltage platform, so it is more stable to be used as a reference electrode, especially for the battery positive and negative electrode voltage monitoring in long cycles. It has obvious advantages. In addition, the reference electrode in the present application is relatively small enough, so the lithium iron phosphate material on the reference electrode is small enough, so that the reference electrode will not have too much impact on the overall capacity balance of the whole battery.

[0008] In one implementation of the present application, the three-electrode soft-pack battery undergoes an activation treatment, and the activation treatment refers to: subjecting the three-electrode soft-pack battery to a charge and discharge cycle, and ultimately making the battery's state of charge 40% to 60%. It should be noted that the three-electrode soft-pack battery of the present application needs to be activated after assembly. Through the activation treatment, the reference electrode can be activated, and the activated three-electrode soft-pack battery can be used for various system tests. It should also be noted that ultimately making the battery in a half-charged state can make the battery system more stable.

[0009] In one implementation of the present application, the area ratio of the diaphragm to the negative electrode sheet is 1.06 to 1.2, and the area ratio of the negative electrode sheet to the positive electrode sheet is 1.05 to 1.1. It should be noted that the diaphragm should completely cover the negative electrode sheet, and the negative electrode sheet should completely cover the positive electrode sheet. In this case, it can be ensured that the electrodes are completely separated by the diaphragm to prevent the positive and negative electrodes from contacting and causing a short circuit. In addition, the area of ​​the negative electrode is larger than that of the positive electrode, which is conducive to making the lithium ion embedding process more uniform, and will not cause uneven potential and cause errors.

[0010] In one implementation of the present application, the reference electrode is located in the middle of the positive electrode sheet and / or the negative electrode sheet. It should be noted that because the area of ​​the negative electrode sheet is larger than that of the positive electrode sheet, in most cases, the edge of the negative electrode sheet is not directly facing the positive electrode sheet, resulting in uneven edges during the lithium ion embedding process, which will lead to uneven potential. In order to avoid the problem of errors caused by such uneven potential, the reference is placed in the center of the positive electrode sheet. When lithium ions are embedded and released, the material reaction in the center is more uniform, so the potential is more realistic and the error is relatively small.

[0011] In one implementation of the present application, the reference electrode is connected to the reference electrode ear through a reference electrode blank area, and the reference electrode blank area refers to an area that does not contain lithium iron phosphate material; the area ratio of the reference electrode to the reference electrode blank area is 0.1 to 0.5.

[0012] The second aspect of the present application discloses a method for preparing a three-electrode soft-pack battery, comprising: assembly: welding the positive electrode tab, the negative electrode tab and the reference electrode tab to the positive electrode sheet, the negative electrode sheet and the reference electrode respectively, stacking the positive electrode sheet, the diaphragm, the reference electrode, the diaphragm and the negative electrode sheet in sequence, and then encapsulating them in a soft-pack shell, injecting electrolyte and sealing; activation treatment: performing charge and discharge cycles to ultimately make the battery's state of charge 40% to 60%.

[0013] In one implementation of the present application, the activation treatment includes: activating the battery: using the positive electrode sheet as the positive electrode and the negative electrode sheet as the negative electrode, performing a charge-discharge cycle, and finally making the battery's state of charge 40% to 60%; activating the reference electrode: including: using the reference electrode as the positive electrode and the negative electrode sheet as the negative electrode, performing a charge-discharge cycle, and finally making the battery's state of charge 40% to 60%; using the positive electrode sheet as the positive electrode and the reference electrode as the negative electrode, performing a charge-discharge cycle, and finally making the battery's state of charge 40% to 60%. It should also be noted that the positive electrode sheet and the negative electrode sheet of the present application can be coated with active slurry on one side.

[0014] In one implementation of the present application, the activated battery includes: the activated battery includes: using a current of 0.08 to 0.12C to charge the battery with a constant current to a cut-off voltage, charging with a cut-off voltage constant voltage until the current is less than 0.05C and then stopping charging, and then discharging with a current of 0.1C to the cut-off voltage and then stopping discharging, after three cycles of charge and discharge, the battery is charged with a current of 0.05C to the cut-off voltage and then stopped charging, and discharged with a current of 0.05C to the cut-off voltage and then stopped discharging, and the last cycle of discharge capacity is used as a reference, and the battery is charged with a current of 0.05C to a state of charge of 40% to 60%. It should be noted that in the present application, a current value of 0.05C is used for activation. Since the current value is small enough, it can significantly reduce polarization, which helps the battery to form a stable SEI film on the negative electrode during the first cycle of charge and discharge, which is convenient for later testing.

[0015] In one implementation of the present application, the activation of the reference electrode includes: making the reference electrode the positive electrode and the negative electrode the negative electrode, first charging and then discharging with a current of 0.05C, wherein the charging is cut off for 18 hours and the discharging is cut off for 18 hours, and the charge and discharge cycle is three cycles, and the discharge capacity of the last cycle is used as a reference, and the reference electrode is charged to a state of charge of 40% to 60% using a current of 0.05C; making the positive electrode sheet the positive electrode and the reference electrode the negative electrode, first discharging and then charging with a current of 0.05C, wherein the discharge is cut off for 18 hours and the charging is cut off for 18 hours, and the charge and discharge cycle is three cycles, and the charge capacity of the last cycle is used as a reference, and finally the reference electrode is discharged to a state of charge of 40% to 60% using a current of 0.05C.

[0016] Regarding the activation treatment of the present application, it should be noted that, in the present application, the battery is first activated so that the battery can be in a half-charged state, and the half-charged battery system is relatively stable, which is convenient for the subsequent activation of the reference electrode; then the lithium iron phosphate material on the reference electrode facing the positive electrode sheet and the lithium iron phosphate material on the reference electrode facing the negative electrode sheet are activated respectively, thereby realizing the activation of the reference electrode; the reference electrode is activated and adjusted to a half-charged state because the voltage platform of the lithium iron phosphate material is very stable when the charge state is between 40% and 60%, and therefore, the voltage stability of the lithium iron phosphate when the charge state is around 50% is utilized, so that it can exist relatively stably as a reference electrode.

[0017] In one implementation of the present application, the state of charge of the battery is 50% after the activation treatment.

[0018] The beneficial effects of this application are:

[0019] The three-electrode soft-pack battery of the present application has a simple structure and is easy and quick to prepare; the reference electrode is activated in advance, and the reference electrode is small, so the impact on the capacity of the whole battery is small; the reference electrode of the present application is stable and suitable for real-time monitoring of the positive and negative electrode voltages during long cycles. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the structure of the three-electrode soft-pack battery involved in this application.

[0021] Figure 2 It is a schematic diagram of the positions of the soft package shell, positive electrode sheet, negative electrode sheet, reference electrode and film involved in this application.

[0022] Figure 3 This is an appearance diagram of the single-layer laminated soft-pack battery of Example 1 of the present application.

[0023] Figure 4 This is a time-voltage variation diagram of the single-layer laminated soft-pack battery of Example 1 of the present application during long-term cycling. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below by specific embodiments in conjunction with the accompanying drawings. In the following embodiments, many detailed descriptions are intended to enable the present application to be better understood. However, those skilled in the art can effortlessly recognize that some of the features can be omitted in different situations, or can be replaced by other materials and methods. In some cases, some operations related to the present application are not shown or described in the specification, in order to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and they can fully understand the related operations according to the description in the specification and the general technical knowledge in the art.

[0025] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate manner to form various implementations. At the same time, the steps or actions in the method description can also be interchanged or adjusted in a manner that is obvious to those skilled in the art. Therefore, the various sequences in the specification and the drawings are only for the purpose of clearly describing a certain embodiment and are not meant to be a required sequence, unless otherwise specified that a certain sequence must be followed.

[0026] The serial numbers assigned to the components in this article, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning.

[0027] With the popularization of new energy vehicles, the performance requirements for lithium-ion batteries are getting higher and higher, and the update and iteration speed of lithium-ion power batteries is getting faster and faster. Therefore, it is particularly important to improve the efficiency of the system evaluation of power batteries. Among the system evaluation methods and evaluation means of lithium-ion power batteries, soft-pack laminated batteries are particularly suitable for early system evaluation because of their simple preparation and ability to basically simulate the actual performance of the full battery system. They are conducive to shortening the test evaluation cycle and improving test efficiency. In recent years, the use of three-electrode batteries to study the potential changes, impedance changes, lithium precipitation behavior, etc. of lithium-ion batteries under different conditions has become an important evaluation method.

[0028] Among the reference electrodes widely used at present, the copper wire reference electrode has the advantages of simple preparation and low cost. However, in actual use, the metal lithium plated on the copper wire of the reference electrode is extremely active and will dissolve in the battery system in a short time at high temperature, which will affect the battery data judgment in the test. At the same time, the copper wire needs to be re-plated with lithium again, which is not suitable for monitoring the positive and negative voltages of long-cycle batteries. Lithium iron phosphate can be used as a stable reference electrode because of its relatively stable lithium deintercalation voltage platform, especially for monitoring the positive and negative voltages of batteries in long cycles. At present, there are also lithium iron phosphate reference electrodes, but the preparation process of the reference electrode is relatively complicated. It is necessary to assemble the whole battery and perform charge and discharge cycles, then take out the lithium iron phosphate sheet for rinsing and drying, and cut the required shape and size to obtain the reference electrode, and then bury the reference electrolysis in the fresh battery, which can then be directly used for testing. However, in the preparation process of the reference electrode, operations such as rinsing, drying, drying, and cutting easily cause the reference material on the electrode to fall off. In addition, due to the extremely thin reference electrode and the brittleness of the lithium iron phosphate electrode itself, it is difficult to cut a complete electrode, because the activated lithium iron phosphate material will fall off the aluminum foil current collector during cutting. At the same time, the manual cutting process has burrs and is easy to pierce the diaphragm, and there are certain difficulties in scale.

[0029] In view of this, the present application creatively proposes a three-electrode soft-pack battery and a preparation method thereof, which has the following advantages:

[0030] This application is a single-layer laminated soft-pack battery, which is easy to prepare and can quickly prepare a full battery for later testing and analysis. There is no need for more complex and costly processes such as multi-layer winding and rolling groove welding.

[0031] In this application, the freshly cut and prepared reference electrode is assembled into a full battery and activated, and the activated battery can be used for testing. This application has a simple method for preparing the battery material system to be evaluated into a full battery, which is highly operable, and the lithium iron phosphate reference electrode does not need to be operated too much during the preparation and activation process, which causes problems such as reference electrode material falling off and cumbersome preparation process.

[0032] In the present application, the whole battery is activated in advance and is in a half-charged state, and the lithium iron phosphate material on the reference electrode is small enough so that it does not cause too much impact on the overall capacity balance of the whole battery.

[0033] The reference electrode of the present application is stable and suitable for real-time monitoring of positive and negative electrode voltages during long cycles.

[0034] The present application is introduced below in conjunction with the accompanying drawings and specific implementation methods.

[0035] The present application relates to a three-electrode soft-pack battery (hereinafter sometimes referred to as a "battery" or "soft-pack battery") and a method for preparing a three-electrode soft-pack battery (hereinafter sometimes referred to as a "preparation method").

[0036] Figure 1 It is a schematic diagram of the structure of the three-electrode soft-pack battery involved in this application.

[0037] like Figure 1 As shown, in a specific embodiment, the three-electrode soft-pack battery may include: a positive electrode tab 1, a negative electrode tab 2, a tab glue 3, a separator 4, a positive electrode sheet 5, a negative electrode sheet 6, a reference electrode tab 7, a reference electrode blank area 8, a reference electrode 9, an aluminum-plastic film 10 (i.e., a soft-pack shell), a positive electrode sheet blank area 11, and a negative electrode sheet blank area 12.

[0038] In a specific embodiment, the positive electrode sheet 5 is an aluminum foil coated with positive electrode sheet slurry.

[0039] In a specific embodiment, the positive electrode sheet 5 is an aluminum foil coated on one side, that is, the side facing the negative electrode sheet 6 is coated with the positive electrode sheet slurry.

[0040] In a specific embodiment, the surface density of the positive electrode sheet 5 is 18.5-22.5 mg / cm 2 .

[0041] In a specific embodiment, the positive electrode slurry is obtained by mixing a positive electrode active material, a conductive agent, polyvinylidene fluoride (PVDF) and nitrogen methyl pyrrolidone (NMP).

[0042] In a specific embodiment, the positive electrode active material can be one or more of lithium iron phosphate, NCM (nickel cobalt manganese ternary material), NCMA (nickel cobalt manganese aluminum quaternary material), NCA (nickel cobalt aluminum ternary material), lithium iron manganese phosphate, lithium manganese oxide, etc.

[0043] In a specific embodiment, the conductive agent may be superconductive carbon (Super-C or carbon nanotube).

[0044] In a specific embodiment, in the positive electrode sheet slurry, by weight, the positive electrode active material is 100 parts, the conductive agent is 2.0-3.0 parts, the polyvinylidene fluoride is 1-2 parts, and the NMP is 55-65 parts.

[0045] In a specific embodiment, in the positive electrode slurry, by weight, lithium iron phosphate: conductive agent: polyvinylidene fluoride: NMP = 100:2.5:1.3:62.

[0046] In a specific embodiment, the negative electrode sheet 6 is a copper foil coated with a negative electrode sheet slurry.

[0047] In a specific embodiment, the negative electrode sheet 6 is an aluminum foil coated on one side, that is, the side facing the positive electrode sheet 5 is coated with the negative electrode sheet slurry.

[0048] In a specific embodiment, the surface density of the negative electrode sheet 6 is 8-11 mg / cm 2 .

[0049] In a specific embodiment, the negative electrode slurry is composed of a negative electrode active material, a conductive agent, carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), H2O (water) and nitrogen-methyl pyrrolidone (NMP).

[0050] In a specific embodiment, the negative electrode active material is one or more of graphite, silicon-oxygen, silicon-carbon, soft and hard carbon, etc.

[0051] In a specific embodiment, in the negative electrode slurry, by weight, the negative electrode active material is 100 parts, the conductive agent is 0.8-1.5 parts, the CMC is 1.2-1.5 parts, the SBR is 3-3.5 parts, the H2O is 80-90 parts, and the NMP is 1 part.

[0052] In a specific embodiment, in the negative electrode slurry, by weight, graphite: conductive agent: CMC: SBR: H2O: NMP = 100:1:1.3:3.2:85:1.

[0053] In a specific embodiment, the reference electrode 9 is an aluminum foil coated with a reference electrode slurry.

[0054] In one embodiment, the reference electrode slurry is the same as the positive electrode slurry.

[0055] In a specific embodiment, the surface density of the reference electrode 9 is 38-45 mg / cm 2 .

[0056] In a specific embodiment, the tab is aluminum foil or copper foil.

[0057] In a specific embodiment, the tab glue 3 is epoxy resin or acrylate.

[0058] In a specific embodiment, the diaphragm 4 is a polyolefin diaphragm, a polyester diaphragm, a non-woven fabric diaphragm or a ceramic diaphragm.

[0059] In a specific embodiment, the positive electrode sheet blank area 11 is an aluminum foil that is not coated with the positive electrode sheet slurry.

[0060] In a specific embodiment, the negative electrode sheet blank area 12 is a copper foil that is not coated with the negative electrode sheet slurry.

[0061] In a specific embodiment, the reference electrode blank area 8 is an aluminum foil that is not coated with the reference electrode slurry.

[0062] Figure 2 It is a schematic diagram of the positions of the soft package shell, positive electrode sheet, negative electrode sheet, reference electrode and film involved in this application.

[0063] In a specific embodiment, if Figure 2 As shown, in the soft-pack battery, the positive electrode sheet 5 , the separator 4 , the reference electrode 9 , the separator 4 , and the negative electrode sheet 6 are stacked in sequence and located between two layers of aluminum-plastic films 10 .

[0064] In a specific embodiment, the three-electrode soft-pack battery is a single-layer laminate soft-pack battery.

[0065] In a specific embodiment, the length and width of the diaphragm 4 are respectively greater than the length and width of the negative electrode sheet 6, the length and width of the negative electrode sheet 6 are respectively greater than the length and width of the positive electrode sheet 5, and the length and width of the positive electrode sheet 5 are respectively greater than the length and width of the reference electrode 9.

[0066] In a specific embodiment, the area ratio of the separator 4 to the negative electrode sheet 6 is 1.06 to 1.2.

[0067] In a specific embodiment, the area ratio of the separator 4 to the negative electrode sheet 6 is 1.08.

[0068] In a specific embodiment, the area ratio of the negative electrode sheet 6 to the positive electrode sheet 5 is 1.05 to 1.1.

[0069] In a specific embodiment, the area ratio of the negative electrode sheet 6 to the positive electrode sheet 5 is 1.08.

[0070] In a specific embodiment, the reference electrode 9 occupies 0.001-0.01 of the area of ​​the positive electrode sheet 5. For example, the reference electrode 9 occupies 0.001, 0.002, 0.004, 0.005, 0.006, 0.008 or 0.01 of the area of ​​the positive electrode sheet 5.

[0071] In a specific embodiment, the reference electrode 9 occupies 0.002-0.05 of the area of ​​the positive electrode sheet 5 .

[0072] In a specific embodiment, the positive electrode sheet 5, the negative electrode sheet 6 and the reference electrode 9 are respectively connected to the positive electrode tab 1, the negative electrode tab 2 and the reference electrode tab 7 through the positive electrode sheet blank area 11, the negative electrode sheet blank area 12 and the reference electrode blank area 8 by ultrasonic welding or electric welding.

[0073] In a specific embodiment, the area ratio of the reference electrode 9 to the reference electrode blank area 8 is 0.1 to 0.5. For example, the area ratio of the reference electrode 9 to the reference electrode blank area 8 is 0.1, 0.2, 0.3, 0.4 or 0.5.

[0074] In a specific embodiment, in the soft-pack battery, the positive electrode sheet 5 is located in the middle of the negative electrode sheet 6 , the negative electrode sheet 6 is located in the middle of the separator 4 , and the reference electrode 9 is located in the middle of the separator 4 .

[0075] In a specific embodiment, the positive electrode tab 1 and the negative electrode tab 2 are respectively located on the left and right sides of the outer surface of the aluminum-plastic film 10 .

[0076] In a specific embodiment, insulating tape can be used to stick the positive electrode blank area 11, the negative electrode blank area 12 and the reference electrode blank area 8 to the film 4 and the aluminum-plastic film 10 respectively, so that the positive electrode 5, the negative electrode 6, the diaphragm 4 and the reference electrode 9 are fixed to the center of the aluminum-plastic film 10.

[0077] In a specific embodiment, the tab glue 3 is respectively sleeved on the positive electrode tab 1 , the negative electrode tab 2 and the reference electrode tab 7 .

[0078] In a specific embodiment, the aluminum-plastic film 10 is filled with electrolyte.

[0079] In a specific embodiment, the solvent in the electrolyte is three or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate.

[0080] In a specific embodiment, the lithium salt in the electrolyte is one or more of LiBF4, LiPF6 and LiBOB.

[0081] In a specific embodiment, the concentration of lithium salt in the electrolyte is 1-1.25 mol / L.

[0082] In a specific embodiment, the electrolyte contains an additive, and the additive may be FEC (fluoroethylene carbonate).

[0083] In a specific embodiment, the mass percentage of the additive in the electrolyte is 1% to 5% (w / w).

[0084] In a specific embodiment, the length or width of the positive electrode sheet 5 is 30-60 mm.

[0085] In a specific embodiment, the length or width of the negative electrode sheet 6 is 32-62 mm.

[0086] In a specific embodiment, the length or width of the diaphragm 4 is 34-64 mm.

[0087] In one embodiment, the soft pack battery is activated.

[0088] In a specific embodiment, the activation treatment step includes: activating the battery and activating the reference electrode.

[0089] In a specific embodiment, activating the battery includes: using the positive side as the positive electrode and the negative side as the negative electrode, using a current of 0.08 to 0.12C to charge the battery at a constant current to a cut-off voltage, charging at a cut-off voltage constant voltage until the current is less than 0.05C and then stopping the charging, then discharging at a current of 0.1C to the cut-off voltage and then stopping the discharging, after three charge and discharge cycles, then charging the battery at a constant current of 0.05C to the cut-off voltage and then stopping the charging, discharging at a constant current of 0.05C to the cut-off voltage and then stopping the discharging, and taking the last discharge capacity as a benchmark, using a current of 0.05C to charge the battery to a state of charge of 40% to 60%.

[0090] In a specific embodiment, activating the reference electrode 9 comprises:

[0091] The reference electrode side is made positive, the negative electrode side is made negative, and the charge and discharge are performed at a current of 0.05C, wherein the charge is terminated for 18 hours and the discharge is terminated for 18 hours, and the charge and discharge cycle is repeated three times. Based on the discharge capacity of the last cycle, the reference electrode is charged to a charge state of 40% to 60% using a current of 0.05C;

[0092] Make the positive electrode side the positive electrode and the reference electrode side the negative electrode, discharge first and then charge with a current of 0.05C, with the discharge period ending at 18h and the charge period ending at 18h, and perform three cycles of discharge and charge. Take the charging capacity of the last cycle as the benchmark, and finally use a current of 0.05C to discharge the reference electrode to a charge state of 40% to 60%.

[0093] In a specific embodiment, the specific preparation method of the three-electrode soft-pack battery can be: the positive electrode sheet 5, the negative electrode sheet 6 and the reference electrode 9 are connected to the positive electrode tab 1, the negative electrode tab 2 and the reference electrode tab 7 by ultrasonic welding through the positive electrode sheet blank area 11, the negative electrode sheet blank area 12 and the reference electrode blank area 8 respectively. According to the order of positive electrode sheet 5-diaphragm 4-reference electrode 9-diaphragm 4-negative electrode sheet 6, they are laid flat and stacked in the middle of the two layers of aluminum-plastic film 10, so that the positive electrode sheet 5 is located in the middle of the negative electrode sheet 6, the negative electrode sheet 6 is located in the middle of the diaphragm 4, and the reference electrode 9 is located in the middle of the diaphragm 4. The positive electrode tab 1 and the negative electrode tab 2 are respectively placed on the left and right sides of the aluminum-plastic film, and finally, insulating tape is used to stick to the positive electrode sheet blank area 11, the negative electrode sheet blank area 12 and the reference electrode sheet blank area 8 respectively, so that the positive electrode sheet 5, the negative electrode sheet 6, the diaphragm 4 and the reference electrode 9 are fixed in the center of the aluminum-plastic film 10. After the electrolyte is injected, the edges of the two layers of aluminum-plastic film 10 are bonded together by vacuum heat sealing to form a closed soft-pack battery. Subsequently, an activation treatment is performed.

[0094] The present application is further described in detail below by specific examples. The following examples are only further described for the present application and should not be construed as limiting the present application. It should be noted that the reagents, test kits, instruments, etc. used in the examples are all commercially available, and the operating steps are carried out according to the instructions or the general operating steps in the art.

[0095] Embodiment 1:

[0096] (1) Material preparation:

[0097] The positive electrode sheet is an aluminum foil coated with a positive electrode slurry on one side. The positive electrode slurry is made of a mixture of lithium iron phosphate, conductive agent (carbon nanotubes), polyvinylidene fluoride (PVDF) and nitrogen methyl pyrrolidone (NMP), where lithium iron phosphate: graphite: PVDF: NMP = 100: 2.5: 1.3: 62; the surface density of the positive electrode sheet is 20 mg / cm 2 After rolling, the die-cutting knife is used to cut the aluminum foil into 54mm in length and 48mm in width using a hydraulic press. The blank area of ​​the positive electrode sheet refers to the aluminum foil that is not coated with the positive electrode sheet slurry, and the length and width are both 10mm.

[0098] The negative electrode sheet is a copper foil coated with negative electrode sheet slurry on one side. The negative electrode sheet slurry is made of a mixture of graphite, conductive agent (carbon nanotubes), carboxymethyl cellulose (CMC), water, styrene-butadiene rubber (SBR) and nitrogen-methyl pyrrolidone (NMP), wherein graphite: carbon black: CMC: SBR: water: NMP = 100:1:1.3:3.2:85:1; the surface density of the negative electrode sheet is 10 mg / cm 2 After rolling, the aluminum foil is cut into 56 mm long and 50 mm wide using a hydraulic press and a die cutter. The negative electrode blank area refers to the aluminum foil that is not coated with the negative electrode slurry, and the length and width are both 10 mm.

[0099] The diaphragm is a polyethylene film with a length of 58 mm and a width of 52 mm;

[0100] The reference electrode is an aluminum foil coated with reference electrode slurry on both sides, and the reference electrode slurry is made of a mixture of lithium iron phosphate, conductive agent (carbon nanotubes), polyvinylidene fluoride (PVDF) and nitrogen methyl pyrrolidone (NMP), wherein lithium iron phosphate: graphite: PVDF: NMP = 100:2.5:1.3:62; only part of the aluminum foil is coated; after rolling, a hydraulic press is used to die-cut the aluminum foil into a length of 38 mm and a width of 1 mm, wherein the area coated with the reference electrode slurry is 8 mm long and 1 mm wide; the area not coated with the reference electrode slurry (reference electrode blank area) is 30 mm long and 1 mm wide.

[0101] The soft package shell is an aluminum-plastic film with a length of 110mm and a width of 80mm.

[0102] Electrolyte: EC (ethylene glycol carbonate): DMC (diethyl carbonate): EMC (ethyl methyl carbonate) = 2:3:5 (volume ratio); the lithium salt is LiPF6, the concentration is 1 mol / L; the additive FEC (fluoroethylene glycol carbonate) is 3% of the total mass of the electrolyte.

[0103] (2) Battery assembly:

[0104] The positive electrode sheet, the negative electrode sheet and the reference electrode are connected to the positive electrode tab, the negative electrode tab and the reference electrode tab by ultrasonic welding through the positive electrode sheet blank area, the negative electrode sheet blank area and the reference electrode blank area, respectively. Then, the positive electrode sheet-diaphragm-reference electrode-diaphragm-negative electrode sheet are laid flat and stacked in the middle of the two layers of aluminum-plastic film (note that the side of the positive electrode sheet coated with the active material and the side of the negative electrode sheet coated with the active material are arranged oppositely), so that the positive electrode sheet is located in the middle of the negative electrode sheet, the negative electrode sheet is located in the middle of the diaphragm, the reference electrode is located in the middle of the diaphragm, and the positive electrode tab and the negative electrode tab are respectively placed on the left and right sides of the aluminum-plastic film. Then, insulating tapes are respectively pasted on the positive electrode sheet blank area, the negative electrode sheet blank area and the reference electrode blank area, so that the positive electrode sheet, the negative electrode sheet, the diaphragm and the reference electrode are fixed to the center of the aluminum-plastic film. Then, the electrolyte is injected, and the injection amount is 1.2g. Finally, the tab glue is respectively put on the positive tab, negative tab and reference electrode tab. The tab glue is 10 mm long and the width is consistent with the width of the positive tab, negative tab and reference electrode tab. The upper edge of the tab glue is fitted with the upper edge of the aluminum-plastic film to protect the tab and insulate. The edges of the two layers of aluminum-plastic film are bonded together by vacuum heat sealing to form a closed soft-pack battery.

[0105] (3) Reference electrode activation:

[0106] First, with the positive side of the whole battery as the positive electrode and the negative side of the whole battery as the negative electrode, use a current of 0.1C to charge the whole battery at a constant current to 3.6V, then charge at a constant voltage of 3.6V until the current is less than 0.05C and cut off the charging, discharge at a constant current of 0.1C to 2.0V and cut off the discharging, cycle the charge and discharge three times, then use a current of 0.05C to charge the whole battery at a constant current to 3.6V and cut off, use a current of 0.05C to discharge at a constant current to 2.0V and cut off, take the discharge capacity of the last cycle as the benchmark, and finally use a current of 0.05C to charge it again until the state of charge (SoC) is adjusted to 50%.

[0107] Then, the reference side of the whole battery is made the positive electrode, and the negative side of the whole battery is made the negative electrode, and it is charged and discharged at a current of 0.05C, wherein the charging is cut off when the voltage is 3.6V, and the discharging is cut off when the voltage is 2.0V. The charge and discharge cycle is repeated three times, and the discharge capacity of the last cycle is used as the benchmark. Finally, it is charged with a current of 0.05C until the state of charge (SoC) is adjusted to 50%.

[0108] Finally, make the positive side of the whole battery the positive electrode, and the reference side of the whole battery the negative electrode, and discharge and then charge with a current of 0.05C, wherein the discharge is cut off when the voltage reaches -0.35V, and the charge is cut off when the voltage reaches 1.4V. The discharge and charge cycle is repeated three times, and the charging capacity of the last cycle is used as the benchmark. Finally, use a current of 0.05C to discharge it until the state of charge (SoC) is adjusted to 50%.

[0109] Figure 3 This is an appearance diagram of a single-layer laminated soft-pack battery in Example 1 of the present application. Figure 4 This is a time-voltage variation diagram of a single-layer laminated soft-pack battery in Example 1 of the present application for a long cycle. Figure 4 It can be seen that the single-layer laminated soft-pack battery of Example 1 has a very high stability in the potential detected by the reference electrode.

[0110] Embodiment 2:

[0111] The positive electrode sheet is 48mm long and 44mm wide; the negative electrode sheet is 50mm long and 46mm wide; the diaphragm is 52mm long and 48mm wide; the aluminum-plastic film is 106mm long and 76mm wide, and the reference electrode is 5mm long and 1mm wide; the length and width of the blank area of ​​the positive electrode sheet and the blank area of ​​the negative electrode sheet are both 8mm, and the length and width of the blank area of ​​the reference electrode is 30mm and 1mm wide; the length of the positive electrode tab and the negative electrode tab are both 45mm long and 10mm wide; the reference electrode tab is 25mm long and 5mm wide.

[0112] The remaining parameters or steps are the same as those in Example 1.

[0113] Embodiment 3:

[0114] The positive electrode sheet is 50mm long and 46mm wide; the negative electrode sheet is 52mm long and 48mm wide; the diaphragm is 54mm long and 50mm wide; the aluminum-plastic film is 106mm long and 76mm wide, and the reference electrode is 6mm long and 2mm wide; the length and width of the blank area of ​​the positive electrode sheet and the blank area of ​​the negative electrode sheet are both 10mm, and the length and width of the reference electrode blank area are 30mm and 2mm wide; the positive electrode tab and the negative electrode tab are both 46mm long and 8mm wide; the reference electrode tab is 28mm long and 8mm wide.

[0115] The remaining parameters or steps are the same as those in Example 1.

[0116] The above contents are further detailed descriptions of the present application in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present application is limited to these descriptions. For ordinary technicians in the technical field to which the present application belongs, several simple deductions or substitutions can be made without departing from the concept of the present application.

Claims

1. A three-electrode soft-pack battery, characterized in that: include: A soft-package shell, an electrolyte, a diaphragm, a positive electrode sheet, a negative electrode sheet and a reference electrode; the electrolyte is sealed in the soft-package shell, the positive electrode sheet, the diaphragm, the reference electrode, the diaphragm and the negative electrode sheet are stacked in sequence and immersed in the electrolyte; the positive electrode sheet, the negative electrode sheet and the reference electrode are respectively connected to the positive electrode tab, the negative electrode tab and the reference electrode tab located outside the soft-package shell; wherein the reference electrode is coated with lithium iron phosphate on both sides, and the area ratio of the reference electrode to the positive electrode sheet is 0.001 to 0.

01.

2. The three-electrode soft-pack battery according to claim 1, characterized in that: The three-electrode soft-pack battery is subjected to activation treatment, wherein the activation treatment refers to: charging and discharging the three-electrode soft-pack battery in cycles, and finally making the battery's state of charge 40% to 60%.

3. The three-electrode soft-pack battery according to claim 1, characterized in that: The area ratio of the separator to the negative electrode sheet is 1.06 to 1.2, and the area ratio of the negative electrode sheet to the positive electrode sheet is 1.05 to 1.

1.

4. The three-electrode soft-pack battery according to claim 1, characterized in that: The reference electrode is located in the middle of the positive electrode sheet and / or the negative electrode sheet.

5. The three-electrode soft-pack battery according to claim 4, characterized in that: The reference electrode is connected to the reference electrode tab via a reference electrode blank area, wherein the reference electrode blank area refers to an area that does not contain lithium iron phosphate material; an area ratio of the reference electrode to the reference electrode blank area is 0.1 to 0.

5.

6. A method for preparing a three-electrode soft-pack battery according to any one of claims 1 to 5, characterized in that: include: Assembling: welding the positive electrode tab, the negative electrode tab and the reference electrode tab to the positive electrode sheet, the negative electrode sheet and the reference electrode respectively, stacking the positive electrode sheet, the diaphragm, the reference electrode, the diaphragm and the negative electrode sheet in sequence, and then encapsulating them in a soft package shell, injecting electrolyte and sealing; Activation treatment: Carry out charge and discharge cycles to eventually make the battery's state of charge 40% to 60%.

7. The preparation method according to claim 6, characterized in that: The activation treatment comprises: Activating the battery: using the positive electrode sheet as the positive electrode and the negative electrode sheet as the negative electrode, performing a charge and discharge cycle, and finally making the battery's state of charge 40% to 60%; Activate the reference electrode: use the reference electrode as the positive electrode and the negative electrode sheet as the negative electrode to perform charge and discharge cycles, and finally make the battery's state of charge 40% to 60%; use the positive electrode sheet as the positive electrode and the reference electrode as the negative electrode to perform charge and discharge cycles, and finally make the battery's state of charge 40% to 60%.

8. The preparation method according to claim 7, characterized in that: The battery activation method comprises: using a current of 0.08-0.12C to charge the battery with a constant current to a cut-off voltage, charging with a cut-off voltage constant voltage until the current is less than 0.05C and then stopping the charging, then discharging with a current of 0.1C to the cut-off voltage and then stopping the discharging, after three charge and discharge cycles, charging the battery with a current of 0.05C to the cut-off voltage and then stopping the charging, discharging with a current of 0.05C to the cut-off voltage and then stopping the discharging, and charging the battery with a current of 0.05C to the cut-off voltage based on the discharge capacity of the last cycle and then stopping the discharging, and charging the battery with a current of 0.05C to a state of charge of 40%-60% again.

9. The preparation method according to claim 8, characterized in that: The activated reference electrode comprises: The reference electrode is used as the positive electrode, and the negative electrode sheet is used as the negative electrode. The electrodes are charged and then discharged at a current of 0.05C. The charging and discharging are performed for 18 hours and 18 hours, respectively. The charging and discharging are repeated three times. The discharge capacity of the last cycle is used as a reference. The reference electrode is charged to a state of charge of 40% to 60% using a current of 0.05C. The positive electrode sheet is used as the positive electrode and the reference electrode is used as the negative electrode. The electrodes are first discharged and then charged at a current of 0.05C. The discharge is stopped for 18 hours and the charge is stopped for 18 hours. The discharge and charge cycles are repeated three times. The charging capacity of the last cycle is used as the reference. Finally, the reference electrode is discharged at a current of 0.05C until the state of charge is 40% to 60%.

10. The preparation method according to claim 6, characterized in that: After the activation treatment, the state of charge of the battery is 50%.

Citation Information

Patent Citations

  • Battery cell for three-electrode test and test method thereof

    CN112909368A

  • Method for testing cycle life of lithium ion battery

    CN115453380A

  • Reference electrode and preparation method and application thereof

    CN116698934A