Zinc ion battery electrolyte and zinc ion battery
By using a dual additive system of sodium sulfonate salt and amide in zinc ion batteries, the problem of shortening of zinc ion batteries is solved, and significant cycle stability and life extension are achieved without affecting the performance of the electrolyte.
Patent Information
- Application Number
- CN202411190101.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The life of zinc ion batteries is shortened due to side reactions caused by zinc dendrites and free water in the negative electrode of zinc, which hinders its large-scale application. Existing additives cannot take into account both side reactions and dendrites, and affects the viscosity and conductivity of the electrolyte.
Using a dual additive system, including sodium sulfonate salt and amide, the zinc ion solvation structure is reconstructed through its synergistic action, reducing the energy barrier of zinc ion desolvation, and alternate adsorption on the surface of zinc negative electrode, regulating zinc ion deposition and inhibiting side reactions and the formation of dendrites.
The cycle stability and life of zinc ion batteries have been significantly improved, extending the cycle life of zinc ion batteries from tens of hours to 1000 hours, and the cumulative capacity reaches 5Ah cm-2, and improving the balun efficiency of the battery.
Smart Images

Figure CN119069840A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of zinc ion batteries and relates to zinc ion battery electrolyte and a zinc ion battery. Background Art
[0002] Lithium-ion batteries have high energy density and high average output voltage, which makes them widely used in electric vehicles, portable electronic devices and other fields. However, lithium-ion battery safety accidents have occurred frequently in recent years, and people's concerns about the safety of lithium-ion batteries have gradually increased. Aqueous zinc-ion batteries have entered people's field of vision due to their low cost, high safety, and environmental friendliness, showing the potential to replace lithium-ion batteries. Zinc metal has a high theoretical capacity (5855mAh cm -3 ;820mAh g -1 ), and low redox potential (-0.763V vs. standard hydrogen electrode (SHE)). Unfortunately, the zinc negative electrode has problems with zinc dendrites and side reactions caused by free water, which shortens the life of zinc ion batteries and hinders the large-scale application of zinc ion batteries. In order to solve these two major problems, on the one hand, it can be modified in the form of improving the zinc ion deposition method, increasing the zinc ion nucleation sites, effectively confining the zinc ion deposition path, uniform interfacial electric field, and forming an electrostatic shielding layer. On the other hand, it can be considered from the perspective of reducing the side reactions of zinc ion batteries, including: reducing free water in the electrolyte and adjusting the solvation structure. Modification of the zinc negative electrode is the most direct and effective modification method, including surface modification of the zinc negative electrode (design of Zn negative electrode, Zn alloy negative electrode, surface modification of Zn negative electrode), and electrolyte optimization (electrolyte salt optimization, electrolyte concentration optimization, additives, co-solvent electrolyte, eutectic electrolyte and gel electrolyte). Among them, modification through electrolyte additives is the simplest and does not increase the extra weight of the battery, which is convenient for large-scale preparation and application. Electrolyte additives can reduce free water or adjust the zinc ion deposition mode and orientation by reconstructing the zinc ion solvation structure, or adsorb on the surface of the zinc negative electrode to prevent some water molecules in the electrolyte from contacting the zinc negative electrode. There are many types of additives reported. Some additives can only work when added in high concentrations, but they will affect the viscosity and conductivity of the electrolyte itself. Some additives can only play a partial role and cannot take into account the two major problems that occur in zinc ion batteries. Therefore, it is very important to study an electrolyte additive that not only has a small amount of addition but can also control the side reactions and dendrite problems that occur in the battery. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a zinc ion battery electrolyte, thereby improving the cycle stability and cycle life of the zinc ion battery.
[0004] The technical solution adopted by the present invention to solve the technical problem is:
[0005] The first aspect of the present invention provides a zinc ion battery electrolyte, which uses zinc salt as solute and water as solvent, and also includes a first additive and a second additive, wherein the first additive is sodium sulfonate salt, the second additive is amide, and the molar ratio of the first additive to the second additive is 5:1 to 1:1.
[0006] The present invention introduces a dual additive system and utilizes the different polarities between the dual additive molecules to not only reconstruct the Zn 2+ Solvation sheath, and the synergistic effect between the two additive molecules reduces the desolvation energy barrier of zinc ions. The difference in adsorption energy of the two additives on the zinc negative electrode surface can achieve the alternating adsorption of the two additives on the zinc negative electrode surface, regulate the uniform deposition of zinc ions, significantly inhibit side reactions and the formation of zinc dendrites, and thus improve the cycle stability and cycle life of zinc ion batteries.
[0007] Furthermore, the molar ratio of the sodium sulfonate salt to the zinc salt is 1:10 to 1:200, preferably 1:10 to 1:100, and more preferably 1:50 to 1:100.
[0008] Furthermore, the volume ratio of the amide to water is 1:10 to 1:200, preferably 1:20 to 1:100, and more preferably 1:20 to 1:50.
[0009] Furthermore, the sodium sulfonate salt is one or more of sodium 3-mercapto-1-propanesulfonate, sodium propanesulfonate, sodium 3-(N-morpholinyl)propanesulfonate, and sodium benzenesulfonate, preferably sodium 3-mercapto-1-propanesulfonate.
[0010] Furthermore, the amide is one or more of N,N-dimethylacetamide, N,N-dimethylformamide, formamide, and acetamide, preferably N,N-dimethylacetamide.
[0011] Furthermore, the zinc salt is one or more of zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate, zinc perchlorate, and zinc acetate, preferably zinc sulfate.
[0012] The second aspect of the present invention provides a zinc ion battery, comprising the zinc ion battery electrolyte. The positive electrode of the battery is a manganese-based positive electrode, a vanadium-based positive electrode or a Prussian blue positive electrode, and the negative electrode is zinc metal or zinc powder.
[0013] When the electrode area is 1-79.2cm -2 When the Zn-ion battery has a long cycle life and high Coulombic efficiency, the Zn-ion symmetric battery assembled with mixed electrolyte can achieve a high cycle life at 2 mA cm -2 Current density and high areal capacity of 10 mAh cm -2After 1000 hours of cycling, the cumulative capacity reaches 5Ah cm -2 . It is proved that the mixed electrolyte can significantly improve the cycle performance of zinc-ion batteries.
[0014] Advantages and technical effects of the present invention:
[0015] 1. The electrolyte of the present invention introduces a dual additive system, which can work synergistically, not only adsorb alternately on the surface of the zinc negative electrode, but also reduce the zinc deposition energy barrier and improve the zinc ion deposition kinetics. It can significantly inhibit the side reaction and the formation of zinc dendrites, thereby improving the cycle stability and cycle life of the zinc ion battery.
[0016] 2. The present invention can significantly improve the cycle performance of zinc ion button and soft pack batteries, extending the cycle life of zinc ion batteries from 30 hours to 1000 hours, with a cumulative capacity of 5Ah cm -2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Cycling performance diagram of zinc ion symmetric button cell assembled using 1M ZnSO4-0.01M MPS, 1M ZnSO4-0.02M MPS electrolyte and pure ZnSO4 electrolyte prepared in Comparative Example 1;
[0018] Figure 2 Cycling performance diagram of zinc ion symmetric button cell assembled using 1M ZnSO4-2% DMA, 1M ZnSO4-5% DMA electrolyte and pure ZnSO4 electrolyte prepared in Comparative Example 2;
[0019] Figure 3 Cycling performance diagram of zinc ion symmetric button cell assembled using 1M ZnSO4-0.01M MPS / 2%DMA, 1M ZnSO4-0.01M MPS / 5%DMA electrolyte and pure ZnSO4 electrolyte prepared in Example 1;
[0020] Figure 4 Cycling performance diagram of zinc ion symmetric button cell assembled using 1M ZnSO4-0.02M MPS / 2%DMA, 1M ZnSO4-0.02M MPS / 5%DMA electrolyte and pure ZnSO4 electrolyte prepared in Example 2;
[0021] Figure 5 Cycling performance diagram of zinc ion symmetric soft pack battery assembled using 1M ZnSO4-0.01M MPS, 1M ZnSO4-0.02M MPS electrolyte and pure ZnSO4 electrolyte prepared in Comparative Example 1;
[0022] Figure 6Cycling performance diagram of zinc ion symmetric soft pack battery assembled using 1M ZnSO4-2% DMA, 1M ZnSO4-5% DMA electrolyte and pure ZnSO4 electrolyte prepared in Comparative Example 2;
[0023] Figure 7 Cycling performance diagram of zinc ion symmetric soft pack battery assembled using 1M ZnSO4-0.01M MPS / 2%DMA, 1M ZnSO4-0.01M MPS / 5%DMA electrolyte and pure ZnSO4 electrolyte prepared in Example 1;
[0024] Figure 8 Cycling performance diagram of zinc ion symmetric soft pack battery assembled using 1M ZnSO4-0.02M MPS / 2%DMA, 1M ZnSO4-0.02M MPS / 5%DMA electrolyte and pure ZnSO4 electrolyte prepared in Example 2;
[0025] Fig. 9 The 1M ZnSO4-0.02M MPS / 2% DMA electrolyte prepared in Example 2 is used to assemble a zinc ion symmetric soft pack battery test run;
[0026] Fig.10 The 1M ZnSO4-0.02M MPS / 2% DMA electrolyte prepared in Example 2 is used to assemble a zinc ion symmetric button-type asymmetric cell coulombic efficiency performance diagram;
[0027] Fig.11 The pure ZnSO4 electrolyte prepared in Example 2 is used to assemble the zinc ion symmetric soft pack battery test. The scanning electron microscope image of the zinc surface, wherein (a) is a scanning electron microscope image of 10 μm after several dozen hours of circulation, and (b) is a scanning electron microscope image of 1 μm after several dozen hours of circulation;
[0028] Fig.12 The 1M ZnSO4-0.02M MPS / 2% DMA electrolyte prepared in Example 2 is used to assemble the zinc ion symmetric soft pack battery after testing, wherein (a) is a 10 μm scanning electron microscope image after 1000 hours of cycling, and (b) is a 1 μm scanning electron microscope image after 1000 hours of cycling;
[0029] Fig.13 XRD pattern of zinc surface after testing of 1M ZnSO4-0.02M MPS / 2% DMA electrolyte prepared in Example 2 for assembling zinc ion symmetric soft pack batteries. DETAILED DESCRIPTION
[0030] The following will further explain in detail how the MD-ZnSO4 mixed electrolyte improves the cycle life and capacity of zinc ion batteries in conjunction with the accompanying drawings.
[0031] Comparative Example 1:
[0032] Add 5.7512 g of zinc sulfate heptahydrate to 20 mL of deionized water and stir for one hour to obtain pure 1 M (mol -1 )ZnSO4 electrolyte.
[0033] 5.7512 g of zinc sulfate heptahydrate and 0.42 g of sodium 3-mercapto-1-propanesulfonate were added to 20 mL of deionized water, stirred for one hour, and mixed evenly to obtain a 1 M ZnSO4-0.01 M MPS electrolyte.
[0034] 5.7512 g of zinc sulfate heptahydrate and 1.1 g of sodium 3-mercapto-1-propanesulfonate were added to 20 mL of deionized water, stirred for one hour, and mixed evenly to obtain a 1 M ZnSO4-0.02 M MPS electrolyte.
[0035] 1M ZnSO4-0.01M MPS, 1M ZnSO4-0.02M MPS, and 1M ZnSO4 electrolytes were used in assembled zinc ion button cells and soft pack cells, respectively, at a current density of 2mAcm -2 , with a surface capacity of 10 mAh cm -2 Symmetrical battery performance test was performed under operation.
[0036] Figure 1 The button cells of the prepared single electrolyte 1M ZnSO4-0.01M MPS, 1M ZnSO4-0.02M MPS and ordinary zinc sulfate electrolyte were tested at 2mA cm -2 , 10mAh cm -2 As can be seen from the figure, the performance of the battery with a single additive is better than that of the ordinary zinc sulfate electrolyte.
[0037] Figure 5 The soft-pack batteries of the prepared single electrolyte 1M ZnSO4-0.01M MPS, 1M ZnSO4-0.02M MPS and ordinary zinc sulfate electrolyte were tested at 2mA cm -2 , 10mAh cm -2 For large-area soft-pack batteries, the battery performance is a test. As can be seen from the figure, although the battery with a single additive can extend the battery's operating time, the effect is still limited.
[0038] Comparative Example 2:
[0039] Add 5.7512 g of zinc sulfate heptahydrate to 20 mL of deionized water and stir for one hour to obtain pure 1 M (mol -1)ZnSO4 electrolyte.
[0040] 5.7512 g of zinc sulfate heptahydrate and 0.42 g of N,N-dimethylacetamide were added to 20 mL of deionized water, stirred for one hour, and mixed evenly to obtain a 1 M ZnSO4-2% DMA electrolyte.
[0041] 5.7512 g of zinc sulfate heptahydrate and 1.1 g of N,N-dimethylacetamide were added to 20 mL of deionized water, stirred for one hour, and mixed evenly to obtain a 1 M ZnSO4-5% DMA electrolyte.
[0042] 1M ZnSO4-2% DMA, 1M ZnSO4-5% DMA, and 1M ZnSO4 electrolytes were used in assembled zinc ion button cells and soft pack cells, respectively, at a current density of 2 mA cm -2 , with a surface capacity of 10 mAh cm -2 Symmetrical battery performance test was performed under operation.
[0043] Figure 2 The button cells prepared for single electrolyte 1M ZnSO4-2% DMA, 1M ZnSO4-5% DMA and common zinc sulfate electrolyte were tested at 2 mA cm -2 , 10mAh cm -2 As can be seen from the figure, the performance of the battery with a single additive is better than that of the ordinary zinc sulfate electrolyte, but not as good as that of the single MPS additive.
[0044] Figure 6 The prepared single electrolyte 1M ZnSO4-2% DMA, 1M ZnSO4-5% DMA and ordinary zinc sulfate electrolyte soft pack battery at 2mA cm -2 , 10mAh cm -2 As can be seen from the figure, the performance of the battery with a single additive is almost the same as that of the ordinary zinc sulfate electrolyte, proving that the effect of a single additive is limited.
[0045] Embodiment 1:
[0046] Add 5.7512 g of zinc sulfate heptahydrate to 20 mL of deionized water and stir for one hour to obtain pure 1 M (mol -1 )ZnSO4 electrolyte.
[0047] Add 5.7512 g of zinc sulfate heptahydrate, sodium 3-mercapto-1-propanesulfonate and N,N-dimethylacetamide (the molar ratio of sodium 3-mercapto-1-propanesulfonate to N,N-dimethylacetamide is 5:2) into 20 mL of deionized water, stir for one hour, mix well, and obtain 1 M ZnSO4-0.01 M MPS / 2% DMA electrolyte.
[0048] Add 5.7512 g of zinc sulfate heptahydrate, sodium 3-mercapto-1-propanesulfonate and N,N-dimethylacetamide (the molar ratio of sodium 3-mercapto-1-propanesulfonate to N,N-dimethylacetamide is 1:1) into 20 mL of deionized water, stir for one hour, mix well, and obtain 1 M ZnSO4-0.01 M MPS / 5% DMA electrolyte.
[0049] 1M ZnSO4-0.01M MPS / 2% DMA, 1M ZnSO4-0.01M MPS / 5% DMA, and 1M ZnSO4 electrolytes were used in assembled zinc ion button cells and soft pack cells, respectively, at a current density of 2mAcm -2 , with a surface capacity of 10 mAh cm -2 Symmetrical battery performance test was performed under operation.
[0050] Figure 3 The button cells of the prepared mixed electrolyte 1M ZnSO4-0.01M MPS / 2% DMA, 1M ZnSO4-0.01M MPS / 5% DMA and ordinary zinc sulfate electrolyte were tested at 2 mA cm -2 , 10mAh cm -2 As can be seen from the figure, the performance of the battery with mixed electrolyte is much better than that of ordinary zinc sulfate electrolyte, and is also better than that of single MPS and DMA additives.
[0051] Figure 7 The soft-pack batteries of the prepared mixed electrolyte 1M ZnSO4-0.01M MPS / 2% DMA, 1M ZnSO4-0.01M MPS / 5% DMA and ordinary zinc sulfate electrolyte were tested at 2mAcm -2 , 10mAh cm -2 The test performance. As can be seen from the figure, the performance of the battery with mixed electrolyte is much better than that of ordinary zinc sulfate electrolyte, and is also better than the single MPS and DMA additives. It can be seen from the figure that the effect is better when the amount of DMA added is smaller.
[0052] Embodiment 2:
[0053] Add 5.7512 g of zinc sulfate heptahydrate to 20 mL of deionized water and stir for one hour to obtain pure 1 M (mol -1 )ZnSO4 electrolyte.
[0054] Add 5.7512 g of zinc sulfate heptahydrate, sodium 3-mercapto-1-propanesulfonate and N,N-dimethylacetamide (the molar ratio of sodium 3-mercapto-1-propanesulfonate to N,N-dimethylacetamide is 5:1) into 20 mL of deionized water, stir for one hour, mix well, and obtain 1 M ZnSO4-0.02 M MPS / 2% DMA electrolyte.
[0055] Add 5.7512 g of zinc sulfate heptahydrate, sodium 3-mercapto-1-propanesulfonate and N,N-dimethylacetamide (the molar ratio of sodium 3-mercapto-1-propanesulfonate to N,N-dimethylacetamide is 2:1) into 20 mL of deionized water, stir for one hour, mix well, and obtain 1 M ZnSO4-0.02 M MPS / 5% DMA electrolyte.
[0056] 1M ZnSO4-0.02M MPS / 2% DMA, 1M ZnSO4-0.02M MPS / 5% DMA, and 1M ZnSO4 electrolytes were used in assembled zinc ion button cells and soft pack cells, respectively, at a current density of 2mAcm -2 , with a surface capacity of 10 mAh cm -2 Symmetrical battery performance test was performed under operation.
[0057] Figure 4 The button cells of the prepared mixed electrolyte 1M ZnSO4-0.02M MPS / 2% DMA, 1M ZnSO4-0.02M MPS / 5% DMA and ordinary zinc sulfate electrolyte were tested at 2 mA cm -2 , 10mAh cm -2 As can be seen from the figure, the performance of the battery with mixed electrolyte is much better than that of ordinary zinc sulfate electrolyte, and it can be seen that the higher the concentration of MPS, the better the effect.
[0058] Figure 8 The soft-pack cells of the prepared mixed electrolytes 1M ZnSO4-0.02M MPS / 2% DMA, 1M ZnSO4-0.02M MPS / 5% DMA and ordinary zinc sulfate electrolyte were tested at 2 mA cm -2 , 10mAh cm -2As can be seen from the figure, the performance of the battery with mixed electrolyte is much better than that of ordinary zinc sulfate electrolyte. It can be seen that the 0.02M MPS / 2% DMA mixed electrolyte has the best effect, which can allow the soft pack battery to run for 1000 hours, and the cumulative capacity is as high as 5Ah cm -2 .
[0059] Fig. 9 The soft-pack battery of the prepared mixed electrolyte 1M ZnSO4-0.02M MPS / 2% DMA was -2 , 10mAh cm -2 Physical picture of the test run.
[0060] Fig.10 The coulombic efficiency of the button-type asymmetric battery tested for the prepared mixed electrolyte 1M ZnSO4-0.02M MPS / 2% DMA and the ordinary zinc sulfate electrolyte. As can be seen from the figure, ordinary zinc sulfate cannot be tested for a long time in the asymmetric battery test, which indirectly proves the problem of zinc sulfate electrolyte. On the contrary, the use of mixed electrolyte can make the coulombic efficiency of the battery reach more than 98%, proving the excellent performance of the mixed electrolyte.
[0061] Fig.11 This is a scanning electron microscope image of a soft-pack battery prepared with ordinary zinc sulfate electrolyte after operation failure. As can be seen from the image, a large number of dendrites and irregular accumulation appeared on the surface of the zinc foil after operation failure, proving that the use of zinc sulfate electrolyte cannot avoid the side reactions and irregular deposition problems of zinc ion batteries.
[0062] Fig.12 This is a scanning electron microscope image of a soft-pack battery with the prepared mixed electrolyte 1M ZnSO4-0.02M MPS / 2% DMA after the operation was completed. It can be seen from the figure that after the soft-pack battery has been running for 1000 hours, the zinc foil surface deposition is still flat, there is no large-area dendrite problem, and the surface deposition is uniform. It proves that the mixed electrolyte can achieve uniform zinc deposition and reduce the problem of side reactions.
[0063] Fig.13 The XRD diagram of the soft-pack battery after the operation of the prepared mixed electrolyte 1M ZnSO4-0.02M MPS / 2% DMA and the ordinary zinc sulfate electrolyte. It can be seen from the figure that after the soft-pack battery has been running for 1000 hours, the 002 crystal plane on the zinc foil surface is higher than the 100 crystal plane, proving that the mixed electrolyte can adsorb anions on the surface of the zinc negative electrode, which is helpful for the reconstruction of the interface structure and promotes the deposition of zinc ions on the plane.
[0064] To sum up, the above embodiments are only for illustrating relevant principles and implementation methods, and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made to the present invention without departing from the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A zinc ion battery electrolyte, characterized in that: The invention uses zinc salt as solute and water as solvent, and also includes a first additive and a second additive. The first additive is sodium sulfonate salt, the second additive is amide, and the molar ratio of the first additive to the second additive is 5:1 to 1:
1.
2. The zinc ion battery electrolyte according to claim 1, wherein The molar ratio of the sodium sulfonate salt to the zinc salt is 1:10 to 1:
200.
3. The zinc ion battery electrolyte according to claim 1, wherein The volume ratio of the amide to water is 1:10 to 1:
200.
4. The zinc ion battery electrolyte according to claim 1, characterized in that The sodium sulfonate salt is one or more of sodium 3-mercapto-1-propanesulfonate, sodium propanesulfonate, sodium 3-(N-morpholinyl)propanesulfonate and sodium benzenesulfonate.
5. The zinc ion battery electrolyte according to claim 1, characterized in that The amide is one or more of N,N-dimethylacetamide, N,N-dimethylformamide, formamide and acetamide.
6. The zinc ion battery electrolyte according to claim 1, characterized in that The zinc salt is one or more of zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate, zinc perchlorate and zinc acetate.
7. A zinc ion battery, characterized in that: The invention comprises the zinc ion battery electrolyte as described in any one of claims 1 to 4.
8. The zinc ion battery according to claim 7, characterized in that: The positive electrode is a manganese-based positive electrode, a vanadium-based positive electrode or a Prussian blue positive electrode, and the negative electrode is zinc metal or zinc powder.