Recycling method and application of lithium iron phosphate battery

Through the electrochemical method and heat treatment technology of FePO4 materials, the pollution problem in the recycling and treatment of lithium iron phosphate batteries is solved, efficient recycling of battery metals and improved circulation stability, and a safe and economical solution is provided.

CN119069858APending Publication Date: 2024-12-03STATE GRID HUBEI ELECTRIC POWER CO XIAOGAN POWER SUPPLY CO +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411206854.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The economic value of lithium iron phosphate batteries is low, and it is easy to produce hazardous chemicals, leading to environmental pollution, and residual electricity may cause fires, and heavy metal components may cause air and soil pollution.

Method used

The lithium is enriched from the cathode material solution by electrochemical method, and the lithium iron phosphate cathode material is re-prepared by heat treatment to achieve the recycling and utilization of battery metals. Specific steps include electrode pretreatment, preparation of ferric phosphate electrodes, and electrochemical extraction of lithium and regeneration of lithium iron phosphate.

Benefits of technology

It realizes efficient recycling of battery metals, with simple structure and convenient operation, can accurately detect the location of the lesions, provide a better basis for subsequent treatment, and improves the cycle stability and electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069858A_ABST
    Figure CN119069858A_ABST
Patent Text Reader

Abstract

The invention discloses a recovery method and application of a lithium iron phosphate battery, and the method comprises the following steps: step 1, pre-treating an electrode to obtain a lithium-containing electrolyte; step 2, preparation of an iron phosphate electrode: uniformly mixing Fe (NO3) 3.6 H2O and H3PO4 to prepare an aqueous solution, pouring the aqueous solution into a stainless steel reaction kettle with a Teflon lining, carrying out hydrothermal reaction, cooling and removing a solvent to obtain a precursor; then, drying the precursor to obtain iron phosphate, and preparing the iron phosphate into an iron phosphate electrode; 3, electrochemical extraction of lithium: putting an iron phosphate electrode and a graphite plate electrode into the lithium-containing electrolyte, and carrying out electrochemical reaction to obtain lithium; and step 4, regeneration of lithium iron phosphate treatment is carried out, such that a LiFePO4 / C product is obtained. According to the method, lithium in the solution is directly enriched from the positive electrode material solution by using the FePO4 material through an electrochemical method, and the lithiated ferric phosphate material can be prepared into the lithium iron phosphate positive electrode material again through heat treatment, so that the recycling of battery metal is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery recycling, and in particular to a recycling method for lithium iron phosphate batteries. Background Art

[0002] Lithium iron phosphate batteries are widely used in new energy vehicles due to their excellent safety performance and cycle stability; however, scrapped lithium iron phosphate batteries have low economic value for recycling and processing, are prone to produce a large amount of hazardous chemicals, and the residual power in the battery can easily cause a fire. The heavy metal components in the grid and electrodes can cause environmental, air, and soil pollution.

[0003] Therefore, it is necessary to design a recycling method for lithium iron phosphate batteries to overcome the above problems. Summary of the invention

[0004] In order to avoid the above problems, a method for recycling lithium iron phosphate batteries is provided, in which FePO4 material is used to directly enrich lithium in the positive electrode material solution through an electrochemical method, and the lithiated iron phosphate material can be re-prepared into lithium iron phosphate positive electrode material through heat treatment, thereby realizing the recycling of battery metals.

[0005] The present invention provides a method for recycling lithium iron phosphate batteries, comprising the following steps:

[0006] Step 1, electrode pretreatment: disassemble the waste lithium iron phosphate battery, take out the positive electrode, put it into a hydrochloric acid solution for dissolution, then adjust the pH value to near neutral with ammonia water, filter and remove the precipitate, and obtain a lithium-containing electrolyte;

[0007] Step 2, preparation of iron phosphate electrode: 10-15g Fe(NO3)3·6H2O and 1.5-4g H3PO4 are mixed evenly to prepare 60-80ml aqueous solution, poured into a stainless steel reactor lined with Teflon, and hydrothermally reacted at 120-180°C for 16-32h, cooled and the solvent is removed to obtain a precursor; then, the precursor is dried to obtain iron phosphate, and the iron phosphate is prepared into an iron phosphate electrode;

[0008] Step 3, electrochemical extraction of lithium: placing the iron phosphate electrode and the graphite plate electrode into the above-mentioned lithium-containing electrolyte to carry out an electrochemical reaction to obtain lithium;

[0009] Step 4, regeneration of lithium iron phosphate treatment: add LiOH to iron phosphate at a molar ratio of Li to Fe of 1:1, then add sucrose, dry, vacuum dry the dried product, grind it evenly, and calcine it in an inert atmosphere to obtain a LiFePO4 / C product.

[0010] Preferably, in step 2, 11.3 g Fe(NO3)3·6H2O and 2.74 g H3PO4 are mixed evenly to prepare 70 ml of aqueous solution, poured into a stainless steel reactor lined with Teflon, and hydrothermally reacted at 150°C for 24 hours, then naturally cooled to room temperature and the solvent is removed to obtain a precursor; then the precursor is placed in a drying oven at 50-80°C and dried to obtain iron phosphate.

[0011] Preferably, in step 2, the particle size of the iron phosphate is 2 to 3 μm.

[0012] Preferably, in step 2, iron phosphate and acetylene black are uniformly mixed in a mass ratio of 9:1, and then 1% polytetrafluoroethylene emulsion is added to form a uniform paste, which is applied on a conductive nickel mesh and pressed to obtain an iron phosphate electrode.

[0013] Preferably, in step 3, the iron phosphate electrode is connected to the working electrode of the constant potential instrument, the graphite electrode is connected to the counter electrode, a silver / silver chloride electrode is used as a reference electrode, and the iron phosphate electrode is discharged at a constant current of 50 mA per 60-90 grams of iron phosphate, and the discharge cut-off potential is -0.5 V to extract lithium.

[0014] Preferably, in step 4, the baking is carried out in a water bath at 70-90° C., the calcination temperature is 600-700° C., and the calcination time is 8-12 h.

[0015] Preferably, in step 4, the inert atmosphere is N2-5% H2.

[0016] Preferably, the recovered LiFePO4 / C product is used to prepare a lithium battery.

[0017] Compared with the prior art, the present invention has the following beneficial effects: the lithium iron phosphate battery recycling method is simple in structure, convenient in operation, flexible and practical, and can accurately detect the size and location of lesions, providing better preparation and more accurate basis for subsequent treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a SEM image of the iron phosphate obtained in a preferred embodiment of the present invention;

[0019] Figure 2 XRD diffraction patterns of LiFePO4 / C products obtained by calcining the precursors obtained by hydrothermal treatment at 130°C (C / LFP-130) and 180°C (C / LFP-180) for 6h at high temperature in a preferred embodiment of the present invention;

[0020] Figure 3 This is a TEM photo of carbon-coated LiFePO4 particles obtained at 180°C for 6h in a preferred embodiment of the present invention;

[0021] Figure 4The charge and discharge curves of C / LFP-130 and C / LFP-180 at current densities of 0.3C, 0.5C, and 1C, respectively, according to a preferred embodiment of the present invention;

[0022] Figure 5 This is a cycle performance diagram of C / LFP-130 and C / LFP-180 according to a preferred embodiment of the present invention. DETAILED DESCRIPTION

[0023] This embodiment provides a recycling method and application of a lithium iron phosphate battery, which uses FePO4 material to directly enrich lithium in the positive electrode material solution through an electrochemical method, and the lithiated iron phosphate material can be re-prepared into a lithium iron phosphate positive electrode material through heat treatment. The specific recycling steps are as follows:

[0024] Step 1, electrode pretreatment;

[0025] After disassembling the waste lithium iron phosphate battery, taking out the positive electrode, dissolving it in a hydrochloric acid solution, adjusting the pH value to near neutral with ammonia water, filtering to remove the precipitate, and obtaining a lithium-containing electrolyte;

[0026] Step 2, preparation of iron phosphate electrode;

[0027] Mix 11.3g Fe(NO3)3·6H2O and 2.74g H3PO4 evenly to prepare 70ml aqueous solution, pour into 100ml stainless steel reactor with Teflon lining, hydrothermally react at 150℃ for 24h, cool naturally to room temperature, remove all solvents to obtain the precursor. Then, dry the precursor in a drying oven at 60℃ to obtain the target product, iron phosphate. Then, mix iron phosphate and acetylene black in a mass ratio of 9:1, add 1% polytetrafluoroethylene emulsion, adjust to a uniform paste, apply it on a conductive nickel mesh, and press it into an iron phosphate electrode.

[0028] Step 3, electrochemical extraction of lithium;

[0029] Place an iron phosphate electrode and a graphite plate electrode in a tank containing the above-mentioned lithium-containing electrolyte. The iron phosphate electrode is connected to the working electrode of the constant potential instrument, the graphite electrode is connected to the counter electrode, and a silver / silver chloride electrode is used as a reference electrode. The iron phosphate electrode is discharged at a constant current of 50 mA per 83.3 grams of iron phosphate, and the discharge cut-off potential is -0.5V. The iron phosphate material can obtain a capacity of nearly 120 mAh / g, which is equivalent to 0.7 lithium ions embedded in each mole of iron phosphate. If the electrode is updated for repeated extraction, the lithium extraction efficiency can reach more than 98%.

[0030] Step 4, regeneration of lithium iron phosphate treatment;

[0031] LiOH is added to the ferric phosphate in a Li:Fe molar ratio of 1:1, and then 5%-10% sucrose is added, and the mixture is dried in a water bath at 80°C. The dried product is vacuum dried and ground evenly, and then calcined at 650°C for 10 hours in an inert atmosphere (N2-5% H2) to obtain the final LiFePO4 / C.

[0032] The above products were tested for their structure and electrochemical performance:

[0033] A. Structural Characterization

[0034] In order to improve the electronic conductivity of the material, the spherical precursor obtained by the hydrothermal reaction was immersed in a sucrose solution, dried and then calcined at high temperature (650°C, 10h) to obtain carbon-coated spherical LiFePO4. Figure 2 The XRD spectra of the product obtained by high-temperature calcination of the microsphere precursor obtained by hydrothermal synthesis at 130°C (C / LFP-130) and the product obtained by high-temperature calcination of the microsphere precursor obtained at 180°C (C / LFP-180) were compared. As can be seen from the figure, the diffraction spectra of the two samples are basically consistent with the standard spectrum data of LiFePO4 (JCPDF database, card number: 40-1499), and both conform to the characteristics of the orthorhombic system D2h, Pmnb space group, that is, they show the characteristic olivine-type crystal structure. It can be seen that pure olivine-type LiFePO4 can be obtained from the precursors obtained at different hydrothermal temperatures. Calculated by the Debye-Scherer formula, the grain size of C / LFP-130 and C / LFP-180 products is about 80nm, which is the same as the above-mentioned SEM observation ( Figure 1 ).

[0035] Figure 3 TEM image of carbon-coated LiFePO4 particles obtained at 180°C for 6h. It can be seen that C / LiFePO4 is composed of many tiny nano-grains with a grain size of 60-80nm, which is consistent with the XRD calculation. From the high-resolution TEM of a single grain ( Figure 3 b) It can be seen that the surface of the LiFePO4 grain is coated with a layer of carbon about 30 nanometers thick, while the lattice fringes in the inner layer clearly indicate that the core is a LiFePO4 crystal.

[0036] Thermogravimetric data show that the carbon content of C / LFP-130 and C / LFP-180 is 14.24% and 5.79%, respectively. BET surface area test shows that the adsorption isotherm of pure LiFePO4 (180℃, 6h) shows obvious type III, indicating that the pore size of the particles is macroporous; while the desorption isotherms of C / LFP-130 and C / LFP-180 show type IV, and there is an obvious hysteresis loop between the relative pressure of 0.4-0.9, showing obvious mesoporous characteristics. The specific surface areas of LFP, C / LFP-130 and C / LFP-180 are 8.4m 2 ·g -1 、33.4m 2 ·g -1 and 40.0m 2 ·g -1 The results show that the specific surface area of ​​the material increases significantly through the carbon coating pyrolysis process; the large surface area and the special structure of the mesoporous microspheres will be conducive to the penetration and transmission of the electrolyte, so that the material is expected to obtain high electrochemical performance.

[0037] B Electrochemical Characterization

[0038] After mixing and grinding LiFePO4 / C powder and acetylene black evenly, add polytetrafluoroethylene emulsion (active material, acetylene black, polytetrafluoroethylene mass ratio is 80:12:8), add isopropanol and stir to form electrode paste. The prepared electrode paste is rolled into a positive electrode membrane with a thickness of about 0.1mm and good strength using a double roller press. After drying the electrode membrane at 80℃, take a circular membrane with a diameter of 1.0cm and press it on the aluminum collector.

[0039] The above electrode sheet was used as the working electrode, the metal lithium sheet was used as the counter electrode and the reference electrode, the polypropylene microporous membrane was used as the diaphragm, and 1mol / L LiPF6 / EC:DMC:EMC (1:1:1, v / v) (produced by Zhangjiagang Guotai Huarong Chemical New Materials Co., Ltd., LB315 type lithium ion battery electrolyte) was used as the electrolyte. A three-electrode system simulation battery was assembled in a dry glove box filled with Ar gas (Ar%>99.99%, H2O<15ppm, O2<10ppm). The constant current charge and discharge experiment used the Xinwei battery test system with a charge and discharge cut-off voltage of 4.3-2.0V.

[0040] Figure 4 The charge and discharge curves of C / LFP-130 and C / LFP-180 at current densities of 0.3C, 0.5C, and 1C are given, and the charge and discharge performance of LiFePO4 / C mesoporous microspheres is given. -1 ) at a current density of 1.5 mAh g / cm2, the discharge capacities of C / LFP-130 and C / LFP-180 reached 155 mAh g / cm2, respectively. -1and 150mAh·g -1 Even at a current density of 1C, the discharge capacity of C / LFP-130 can still reach 135mAh·g -1 , the capacity of C / LFP-180 can reach 140mAh·g -1 (87% of theoretical capacity), which is significantly higher than ordinary amorphous LiFePO4 nanoparticles.

[0041] Figure 5 The cycling performance diagrams of C / LFP-130 and C / LFP-180 are given. It can be seen from the figure that at a current density of 1C, the discharge capacity of C / LFP-130 can reach 135mAh·g -1 , while the capacity of C / LFP-180 can reach 140mAh·g -1 (87% of theoretical capacity), which shows that both materials can maintain high discharge capacity even at higher current density. Both materials showed very stable cycle performance at 0.3-1C, and no obvious capacity decay was observed after 120 cycles. However, at a current density of >0.5C, C / LFP-180 can release a higher discharge capacity, which may be due to its higher specific surface area. Therefore, it has good cycle stability and long cycle life at different current densities. The standard required 500-cycle lithium battery is regenerated and then increased by 120 cycles, and the estimated life is increased by 24%.

[0042] application

[0043] Since February 2021, a certain unit has adopted a retired power lithium battery energy storage system to achieve peak load regulation of the power grid, charging during off-peak hours and discharging during peak hours. Taking a 5MW / 10MWh retired battery energy storage system as an example, the system efficiency is generally 90%, with cycles per day, and the energy storage system works 300 days a year. The two-part peak electricity price of 10kV and below for general industrial and commercial electricity in Henan Province is 1.264 yuan / kwh, and the off-peak electricity price is 0.392 yuan / kWh. The calculation is as follows based on the annual investment of a 5MW / 10MWh retired battery energy storage system:

[0044] In 2021, the additional sales = 10MWhx1.264 yuan / kWhx90%x300 = 3.4128 million yuan; the additional profit = 10MWhx90%x300x(1.264 yuan / kWh-0.392 yuan / kwh) = 2.3544 million yuan. In 2022, the additional sales = 20MWhx1.264 yuan / kWhx90%x300 = 6.8256 million yuan; the additional profit = 20MWhx90%x300x(1.264 yuan / kWh-0.392 yuan / kWh) = 4.7088 million yuan. In 2023, the new sales = 30MWh x 1.264 yuan / kWh x 90% x 300 = 10.2384 million yuan; the new profit = 30MWh x 90% x 300 x (1.264 yuan / kWh-0.392 yuan / kwh) = 7.0632 million yuan. Replacing new lithium batteries with retired lithium batteries saves a lot of costs, increases the company's profits in energy storage, enhances the company's ability to absorb new energy, improves power supply reliability and quality, and has significant application effects.

[0045] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for recycling lithium iron phosphate batteries, characterized in that: The steps include: Step 1, electrode pretreatment: disassemble the waste lithium iron phosphate battery, take out the positive electrode, put it into a hydrochloric acid solution for dissolution, then adjust the pH value to near neutral with ammonia water, filter and remove the precipitate, and obtain a lithium-containing electrolyte; Step 2, preparation of iron phosphate electrode: 10-15g Fe(NO3)3·6H2O and 1.5-4g H3PO4 are mixed evenly to prepare 60-80ml aqueous solution, poured into a stainless steel reactor lined with Teflon, and hydrothermally reacted at 120-180°C for 16-32h, cooled and the solvent is removed to obtain a precursor; then, the precursor is dried to obtain iron phosphate, and the iron phosphate is prepared into an iron phosphate electrode; Step 3, electrochemical extraction of lithium: placing the iron phosphate electrode and the graphite plate electrode into the above-mentioned lithium-containing electrolyte to carry out an electrochemical reaction to obtain lithium; Step 4, regeneration of lithium iron phosphate treatment: add LiOH to iron phosphate at a molar ratio of Li to Fe of 1:1, then add sucrose, dry, vacuum dry the dried product, grind it evenly, and calcine it in an inert atmosphere to obtain a LiFePO4 / C product.

2. The method for recycling lithium iron phosphate batteries as claimed in claim 1, characterized in that: In step 2, 11.3 g Fe(NO3)3·6H2O and 2.74 g H3PO4 are mixed evenly to prepare 70 ml of aqueous solution, poured into a stainless steel reactor lined with Teflon, and hydrothermally reacted at 150°C for 24 hours. Then, it is naturally cooled to room temperature and the solvent is removed to obtain a precursor; then the precursor is placed in a drying oven at 50-80°C and dried to obtain iron phosphate.

3. The method for recycling lithium iron phosphate batteries as claimed in claim 1, characterized in that: In step 2, the particle size of the iron phosphate is 2 to 3 μm.

4. The method for recycling lithium iron phosphate batteries as claimed in claim 1, characterized in that: In step 2, iron phosphate and acetylene black are mixed evenly in a mass ratio of 9:1, and then 1% polytetrafluoroethylene emulsion is added to form a uniform paste, which is applied on a conductive nickel mesh and pressed to obtain an iron phosphate electrode.

5. The method for recycling lithium iron phosphate batteries as claimed in claim 1, characterized in that: In step 3, the iron phosphate electrode is connected to the working electrode of the constant potential instrument, the graphite electrode is connected to the counter electrode, and the silver / silver chloride electrode is used as the reference electrode. The iron phosphate electrode is discharged at a constant current of 50 mA per 60-90 grams of iron phosphate, and the discharge cut-off potential is -0.5 V to extract lithium.

6. The method for recycling lithium iron phosphate batteries as claimed in claim 1, characterized in that: In step 4, the mixture is dried in a water bath at 70-90° C., the calcination temperature is 600-700° C., and the calcination time is 8-12 hours.

7. The method for recycling lithium iron phosphate batteries as claimed in claim 1, characterized in that: In step 4, the inert atmosphere is N2-5% H2.

8. The recycling application of lithium iron phosphate batteries as claimed in claim 1, characterized in that: The recovered LiFePO4 / C product is used to prepare lithium batteries.