Semiconductor laser element and light-emitting device

By introducing a stress release layer into the semiconductor laser element, the interface defects and polarization field problems caused by the lattice difference between InGaN and GaN are solved, the carrier recombination efficiency and the stability of the laser are improved, and the bimodal phenomenon is avoided, so as to achieve Better performance.

CN119070137AActive Publication Date: 2024-12-03XIAMEN SANAN OPTOELECTRONICS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411088858.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-03
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

In gallium nitride-based blue-green lasers, the interface defects and polarization field problems are caused by the difference in lattice between InGaN and GaN, which affects the quality stability of the device and the carrier recombination efficiency, resulting in bimodal phenomena and performance degradation.

Method used

In the structure of the semiconductor laser element, the stress release layer is introduced, and by inserting the stress release layer between the first waveguide layer and the active layer, including the In component, the peak intensity of the ion intensity curve of the In component is controlled to be smaller than that of the first waveguide layer. The content of In component is reduced, the lattice distortion rate is improved, the lattice matching degree is improved, and the laser wavelength and carrier recombination position are precisely controlled.

Benefits of technology

It effectively reduces carrier overflow, improves carrier recombination efficiency and gain effect, avoids the occurrence of bimodal phenomena, and improves the performance and stability of the laser.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119070137A_ABST
    Figure CN119070137A_ABST
Patent Text Reader

Abstract

According to the semiconductor laser element and the light-emitting device provided by the invention, the stress release layer is inserted between the first waveguide layer and the active layer, so that the lattice constant is better transited from the substrate layer to the active layer, the lattice distortion rate is reduced, the interlayer lattice matching degree is improved, a better growth environment is provided for the active layer, and the light-emitting efficiency of the semiconductor laser element is improved. Micro-pit defects on the surface of the active layer are reduced, and the crystal quality of the active layer is improved; meanwhile, the peak intensity of the In component in the stress release layer is smaller than the content of the In component in the first waveguide layer, so that the laser wavelength and the carrier recombination position are accurately controlled, electron overflow is reduced, the carrier recombination efficiency and the gain effect are improved, the double-peak phenomenon is avoided, and finally the purpose of improving the light emitting brightness is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a semiconductor laser element and a light-emitting device. Background Art

[0002] III-group nitrides represented by gallium nitride are direct-transition wide-bandgap semiconductor materials with a wide energy band, making them ideal materials for making lasers from the ultraviolet band to the green band. GaN-based blue-green lasers have the advantages of small size, high integration, high brightness, and high resolution. The distribution of the light field and the ability to confine photons are key factors affecting the performance of GaN-based blue-green lasers.

[0003] In laser products, in order to improve the confinement factor and reduce the problem of laser being doped and absorbed in the waveguide layer, the structural design of laser products is simpler than the traditional LED epitaxial structure. The waveguide layer of laser products can be used to limit the light field. When the waveguide layer is made of InGaN material, due to the large difference in the lattice between InGaN and GaN, interface defects are easily formed at the interface between the waveguide layer and the GaN layer. These interface defects will affect the quality stability of the device; at the same time, lattice constant mismatch will also bring about polarization field problems. Carriers cannot recombine more effectively in the quantum well layer, seriously affecting the carrier recombination efficiency; in addition, the polarization field will also cause the carrier recombination position to shift, thereby producing a twin peak phenomenon. The above defects will have a significant negative impact on the performance of laser products.

[0004] Therefore, it is necessary to provide an improved technical solution to address the deficiencies in the above-mentioned prior art. Summary of the invention

[0005] In view of the above defects and deficiencies in the prior art, the purpose of the present application is to provide a semiconductor laser element and a light-emitting device to solve one or more of the above problems.

[0006] According to one aspect of the present application, a semiconductor laser element is provided, comprising at least:

[0007] A semiconductor stack, wherein the semiconductor stack comprises a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence; the first semiconductor layer comprises a first waveguide layer, the second semiconductor layer comprises a second waveguide layer, and the first waveguide layer and the second semiconductor layer are both located on a side of the corresponding semiconductor layer close to the active layer; wherein,

[0008] A stress release layer is also included between the first waveguide layer and the active layer, at least part of the stress release layer contains an In component, and the In component forms an ion intensity curve along the growth direction of the semiconductor stack. The peak intensity of the In component in the stress release layer in the ion intensity curve is less than the In component content in the first waveguide layer.

[0009] According to one aspect of the present application, the present application also provides a semiconductor laser element, comprising at least:

[0010] A semiconductor stack, wherein the semiconductor stack comprises a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence; the first semiconductor layer comprises a first waveguide layer, the second semiconductor layer comprises a second waveguide layer, and the first waveguide layer and the second semiconductor layer are both located on a side of the corresponding semiconductor layer close to the active layer; wherein,

[0011] A stress release layer is further included between the first waveguide layer and the active layer, wherein the stress release layer includes a first sublayer, a second sublayer and an intermediate layer located between the first sublayer and the second sublayer, the intermediate layer contains an In component, and the thickness of the intermediate layer is between The thickness of the stress release layer is between between.

[0012] According to one aspect of the present application, the present application also provides a light-emitting device, which includes the semiconductor laser element described in the above technical solution.

[0013] Compared with the prior art, the semiconductor laser element and light-emitting device provided by the present application have at least the following beneficial effects:

[0014] In the technical solution of the present application, by inserting a stress release layer between the first waveguide layer and the active layer, the lattice constant can be better transitioned from the substrate layer to the active layer, the lattice distortion rate can be reduced, the interlayer lattice matching degree can be improved, a better growth environment can be provided for the active layer, the micro-pit defects on the surface of the active layer can be reduced, and the crystal quality of the active layer can be improved; at the same time, the peak intensity of the In component in the stress release layer is limited to be less than the In component content in the first waveguide layer, so as to accurately control the laser wavelength and the carrier recombination position, reduce electron overflow, improve the carrier recombination efficiency and gain effect, and avoid the double peak phenomenon.

[0015] In addition, the light-emitting device provided in the present application includes the semiconductor laser element provided by the above technical solution, so the light-emitting device also has the above good technical effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. The positional relationships described in the drawings in the following description are based on the directions in which the components are drawn in the diagrams, unless otherwise specified.

[0017] For the purpose of convenience or clarity, the thickness and size of each layer shown in the drawings can be exaggerated, omitted or roughly drawn. In addition, the size of the light emitting device does not completely reflect the actual size.

[0018] Figure 1 A schematic diagram showing a cross-sectional structure of a semiconductor laser element provided by an embodiment of the present application;

[0019] Figure 2 Shown is a schematic cross-sectional structure diagram of a stress release layer provided in one embodiment of the present application;

[0020] Figure 3 A diagram showing the relationship between element ion intensity and depth in a partial range of a semiconductor laser element provided by an embodiment of the present application;

[0021] Figure 4 Display as Figure 3 A partial enlarged schematic diagram of .

[0022] List of reference numerals:

[0023] 100 substrates

[0024] 210 Buffer layer

[0025] 220 First coating layer

[0026] 230 Electronic supply layer

[0027] 240 First waveguide layer

[0028] 250 Stress relief layer

[0029] 251 First Sublayer

[0030] 252 Second Sublayer

[0031] 253 Middle Layer

[0032] 300 Active layer

[0033] 410 Second waveguide layer

[0034] 420 Electron blocking layer

[0035] 430 Second coating layer

[0036] 440 Ohm contact layer

[0037] 500 Contact Electrode

[0038] 600 Insulation

[0039] 700 Second electrode

[0040] 800 First Electrode DETAILED DESCRIPTION

[0041] The following specific embodiments illustrate the implementation of the present application, and those familiar with the technology can easily understand other advantages and effects of the present application from the content disclosed in this specification. The present application can also be implemented or applied through other different specific implementations, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.

[0042] The composition and dopant of each layer included in the semiconductor laser device of the present application can be analyzed by any suitable method, such as secondary ion mass spectrometer (SIMS). The thickness of each layer included in the semiconductor laser device of the present application can be analyzed by any suitable method, such as transmission electron microscopy (TEM) or scanning electron microscopy (SEM), for example, to match the depth position of each layer on the SIMS map.

[0043] In this application, unless otherwise specified, the term "peak shape" refers to a line profile comprising two line segments with slopes of opposite signs, i.e., one line segment has a positive slope and the other line segment has a negative slope. "Peak concentration" refers to the highest concentration value between the two line segments of the peak shape with slopes of opposite signs.

[0044] For ease of description, the growth direction of the semiconductor stack is defined as upward, and the opposite direction is defined as downward.

[0045] like Figure 1-2As shown, this embodiment provides a semiconductor laser element, which includes at least a substrate 100 and a semiconductor stack located above the substrate 100, and the semiconductor stack includes a first semiconductor layer, an active layer 300 and a second semiconductor layer stacked in sequence; the first semiconductor layer in this embodiment is an N-type semiconductor layer, and the second semiconductor layer is a P-type semiconductor layer. The semiconductor laser element is an end-face emitting laser element having a light emitting end face and a light reflecting end face intersecting with the main surface of the semiconductor layer such as the active layer 300, and the semiconductor stack has a ridge of a mesa structure at the top, and the ridge is formed in the second cladding layer 430 of the second semiconductor layer and above, and the extension direction of the ridge is the propagation direction of the laser. An insulating layer 600 is provided on the side of the ridge and on the surface of the second semiconductor layer continuous from the side of the ridge.

[0046] The substrate 100 has a relative upper surface and a lower surface, and a first electrode 800 is provided on the lower surface thereof, and the first electrode 800 forms an electrical contact with the first semiconductor layer. In addition, a contact electrode 500 is provided on the upper surface of the ridge, and the contact electrode 500 forms an ohmic contact with the second semiconductor layer. The semiconductor laser element also includes a second electrode 700 provided on the upper surface of the contact electrode 500, and the second electrode 700 forms an electrical connection with the contact electrode 500. The first electrode 800 and the second electrode 700 act together on the PN junction, and release energy and generate photons through the recombination of electrons and holes. These photons are reflected and amplified by the resonant cavity to form a laser beam, thereby realizing the laser emission function of the laser diode.

[0047] Continue to see Figure 1-2 , the substrate 100 can be a growth substrate, including but not limited to nitride semiconductors, SiC or high-impedance substrates such as sapphire substrates. The substrate containing nitride semiconductors can improve the heat dissipation efficiency because the thermal conductivity is higher than that of sapphire, thereby reducing defects such as dislocations and achieving good crystallinity. In an optional embodiment, the substrate 100 can be a supporting substrate, and the growth substrate originally used for epitaxial growth of the semiconductor stack can be selectively removed according to the needs of the application, and then the semiconductor stack is transferred to the aforementioned supporting substrate. Furthermore, the thickness of the substrate 100 ranges from 40μm to 400μm, for example 50μm, 80μm, 100μm, 150μm, 200μm and 300μm.

[0048] Continue to see Figure 1-2 The first semiconductor layer can be configured as a multilayer structure composed of nitride semiconductors such as GaN, InGaN, and AlGaN. The first semiconductor layer includes a buffer layer 210, a first cladding layer 220, an electron supply layer 230, a first waveguide layer 240, and a stress release layer 250 stacked in sequence on the substrate 100. The first semiconductor layer can also be configured with other layers in addition to the above layers, and a part of the layers can also be omitted.

[0049] In one embodiment, a buffer layer 210 is formed on the substrate 100. The buffer layer 210 is located between the substrate 100 and the first cladding layer 220. The buffer layer 210 is an n-type material layer made of GaN-based III-V nitride semiconductor, or an undoped material layer, and its material may be InGaN, which is used to adjust the substrate warping to improve wavelength uniformity.

[0050] In one embodiment, a first cladding layer 220 is formed on the buffer layer 210. The first cladding layer 220 is located between the buffer layer 210 and the electron supply layer 230 or the first waveguide layer 240. The material of the first cladding layer 220 may be AlGaN. By adjusting the refractive index and thickness of the first cladding layer 220, the light field is limited so that the light field is mainly concentrated between the waveguide layers of the laser for gain, thereby improving the efficiency and performance of the laser. The first cladding layer 220 needs to have a certain thickness to effectively limit carriers and prevent electron overflow. The thickness is usually between 100nm and 500nm.

[0051] In one embodiment, an electron supply layer 230 is formed on the first cladding layer 220. The electron supply layer 230 is located between the first cladding layer 220 and the first waveguide layer 240. The n-type doping concentration of the electron supply layer 230 is greater than or equal to 3×10 18 atom / cm 3 , which is used to effectively increase the electron injection efficiency and improve the recombination efficiency of carriers in the active layer 300. The thickness of the electron supply layer 230 is less than or equal to 100 nm. Specifically, the thickness of the electron supply layer 230 is between 10 nm and 100 nm, preferably between 10 nm and 50 nm, and the doping concentration is between 8×10 18 atom / cm 3 ~1.5×10 19 atom / cm 3 . The n-type impurity doping concentration of the electron supply layer 230 is generally greater than the n-type impurity doping concentration of the first cladding layer 220. It is understandable that since the laser in the waveguide layer will cause the gain coefficient to decrease due to doping, the carrier recombination efficiency will be affected, which will in turn affect the luminous brightness, and the insertion of the electron supply layer 230 can effectively inject electrons from the first cladding layer 220 into the active layer 300, thereby accumulating sufficient non-equilibrium carrier concentration in the well layer of the active layer 300, optimizing the number and distribution of carriers in the active layer 300, and improving the quantum efficiency of the laser; in addition, the electron supply layer 230 can also limit the diffusion of electrons in the horizontal direction, reduce electron overflow, reduce non-radiative recombination of carriers, and ensure that they are mainly concentrated in the active area, thereby improving the efficiency of the laser.

[0052] In the above embodiment, the thickness of the electron supply layer 230 is less than the thickness of the first waveguide layer 240. The relatively thin electron supply layer 230 can reduce the defects caused by the crystal growth in the layer, ensure good light confinement ability, and provide a relatively flat surface as the growth basis of the first waveguide layer 240, which is conducive to improving the crystal quality of the first waveguide layer 240. The thickness of the electron supply layer 230 is between 10nm and 30nm, for example, it can be 10nm, 15nm, 20nm, 25nm or 30nm. An overly thick layer may cause more defects or stresses to be introduced in the subsequent material deposition process, affecting the reliability and stability of the device, while an overly thin layer cannot withstand the stress or temperature changes in the subsequent process, resulting in the cracking or failure of the layer structure, and requiring higher precision for the doping process. Further, the thickness of the electron supply layer 230 is between 15nm and 25nm, for example, 20nm, to achieve a good balance between the electron supply ability and the quality of the layer structure.

[0053] In the above embodiment, the electron supply layer 230 is a GaN material highly doped with Si, and its doping concentration is greater than the doping concentrations of the first cladding layer 220 and the first waveguide layer 240. By setting a higher Si doping concentration, the electron concentration is increased to ensure sufficient carrier recombination in the active layer 300. For a thinner electron supply layer 230, the doping concentration of the electron supply layer 230 is also greater than the peak doping concentration of the Si element in the stress release layer 250. Specifically, the peak doping concentration of the stress release layer 250 is less than or equal to 1.2×10 19 atom / cm 3 , the doping concentration of the electron supply layer 230 is between 8×10 18 atom / cm 3 ~1.5×10 19 atom / cm 3 The doping concentration of the electron supply layer 230 is between 0.1 and 0.2 and greater than that of the stress release layer 250, so as to provide sufficient electrons to the quantum well layer for effective recombination. Furthermore, along the thickness growth direction of the semiconductor stack, the Si element in the electron supply layer 230 is uniformly doped, and the initial doping concentration of the lower surface to the doping concentration of the upper surface is always consistent. The constant doping concentration is conducive to simplifying the preparation process, and also keeps the electron concentration in the electron supply layer 230 stable, which can improve the performance stability of the semiconductor laser element.

[0054] In the above embodiment, a stress release layer 250 is further included between the first waveguide layer 240 and the active layer 300. The stress release layer 250 includes a first sublayer 251, a second sublayer 252 stacked in sequence, and an intermediate layer 253 located between the first sublayer 251 and the second sublayer 252. The intermediate layer contains an In component. For example, the stress release layer can be a GaN / InGaN / GaN multilayer structure. The stress release layer 250 is doped with Si elements. Along the growth direction of the semiconductor stack, the doping concentration of the Si element remains constant or is gradually doped. The stress release layer 250 has at least one doping peak concentration, which is generated in any sublayer in the stress release layer 250, for example, it can be the first sublayer 251, the second sublayer 252 or the intermediate layer 253.

[0055] After testing, under the condition that other semiconductor layer parameters are the same, the thickness of the electron supply layer is 100nm and the doping concentration is 3×10 18 atom / cm 3 The comparison sample and the electron supply layer in this embodiment have a thickness of 20 nm and a doping concentration of 8×10 18 atom / cm 3 For the laser band with a wavelength of 455nm, the limitation factor of the product is increased from 0.71 to 0.74, and the limitation ability of the laser is significantly improved.

[0056] In one embodiment, a first waveguide layer 240 is formed on the electron supply layer 230, and the first waveguide layer 240 is located between the electron supply layer 230 and the stress release layer 250. The material of the first waveguide layer 240 may be InGaN. By doping different proportions of Al components in InGaN, the refractive index and band gap of the waveguide layer are adjusted, so that the refractive index of the first waveguide layer 240 is higher than that of the first cladding layer 220, and the optical signal can be totally reflected at the interface between the waveguide layer and the cladding layer, thereby being confined to propagate in the waveguide layer, achieving an effective optical gain effect. At the same time, the electron supply layer 230 below the first waveguide layer 240 can also play a certain role in reducing electron overflow. The thickness of the first waveguide layer 240 is between 50nm and 500nm to achieve a balance between electron injection efficiency, refractive index and layer structure strength. Further, the thickness of the first waveguide layer 240 is between 200nm and 400nm. In an optional implementation, the In component in the first waveguide layer 240 gradually increases as it approaches the active layer 300 , which can more effectively disperse the deformation of the well layer, improve the crystal quality of the active layer 300 , and increase the carrier recombination efficiency.

[0057] In the above embodiment, the Si doping concentration of the first waveguide layer 240 is lower than the peak doping concentration of the stress release layer 250 , and the Si doping concentration of the first waveguide layer 240 is lower than the doping concentration of the electron supply layer 230 .

[0058] In one embodiment, a stress release layer 250 is formed on the first waveguide layer 240. The stress release layer 250 is located between the first waveguide layer 240 and the active layer 300. Part of the stress release layer 250 contains an In component, such as InGaN. Figure 3 The In component forms an ion intensity curve L along the growth direction of the semiconductor stack, and the peak concentration of the ion intensity curve L is less than the maximum concentration of the In component in the first waveguide layer 240, so as to reduce the lattice defects caused by the lattice constant mismatch, and effectively transfer the lattice constant from the GaN substrate to the InGaN quantum well layer in the active layer 300, which significantly improves the interface flatness of the active layer 300, provides a better growth environment for the quantum well layer, and thus improves the crystal quality of the active layer 300. The setting of the stress release layer 250 can also effectively reduce the influence of the polarization field, increase the hole energy barrier, reduce the overflow probability, and improve the carrier recombination efficiency, while reducing the generation of the peak wavelength twin peak phenomenon. By regulating the material, structure and other process parameters of the stress release layer 250, the quantum well lattice and the polarization field are affected, and then the effective recombination probability and position of the carriers are affected, which can bring good effects on the optoelectronic performance and structural performance of the semiconductor laser. The In content in the thickness of the portion containing the In component in the stress release layer 250 remains constant, or the In component in the stress release layer 250 is uniformly or gradually changed from bottom to top. In an optional embodiment, the thickness of the stress release layer 250 is between Between, for example or If the thickness is too large, the efficiency of carrier injection from the first waveguide layer 240 to the active layer 300 will be affected, resulting in local light absorption, a decrease in the gain coefficient, and a decrease in the brightness of the device; if the thickness is too thin, it will not have an effective lattice constant transition effect and will not have a good stress release effect. Further, the thickness of the stress release layer 250 is between In order to achieve a more balanced stress release effect.

[0059] The stress release layer 250 is doped with Si elements to reduce the polarization field of the active layer 300 and thus increase the recombination efficiency of electrons and holes. The doping concentration is between 5×10 18 atom / cm 3 ~1×10 19 atom / cm 3 At the same time, the Si doping concentration of the electron supply layer 230 is greater than the doping concentration of the stress release layer 250, and its doping concentration is between 8×10 18 atom / cm 3 ~5×10 19 atom / cm 3In an optional embodiment, the Si doping concentration of the electron supply layer 230 is less than or equal to the doping concentration of the stress release layer 250, and the doping concentration of the electron supply layer 230 is adjusted accordingly according to the crystal quality of the waveguide layer.

[0060] The stress release layer 250 includes a first sublayer 251, a second sublayer 252, and an intermediate layer 253 located between the first sublayer 251 and the second sublayer 252, wherein the first sublayer 251 contacts the first waveguide layer 240, the second sublayer 252 contacts the active layer 300, and the intermediate layer 253 contains an In component. The thickness of the intermediate layer 253 is between 100 and 100 nm. In an optional embodiment, the first sublayer 251 and the second sublayer 252 include GaN, the middle layer 253 includes InGaN, and the stress release layer 250 forms a GaN / InGaN / GaN stacked structure, that is, the peak concentration of the ion intensity curve L brought by the In component is generated at the middle layer 253, and the peak concentration of the In ion intensity curve of the InGaN material in the middle layer 253 is less than the maximum concentration of the In component in the first waveguide layer 240. If the In component content of the middle layer 253 is too high, it is easy to cause a double peak phenomenon, the laser wavelength half width becomes larger, the gain effect is poor, and the electron overflow reduces the recombination efficiency, affecting the brightness of the laser product; the In component content of the middle layer 253 is relatively lower than the In ion peak intensity of the first waveguide layer 240, which can reduce lattice mismatch and reduce structural defects. The lower In component content of the middle layer 253 also means that the lattice constant of the layer is closer to that of the second sublayer 252 and the first well layer of the active layer 300, which is more conducive to achieving the stress release effect from the N-type semiconductor layer to the active layer 300. The In component content of the middle layer 253 is kept constant from bottom to top, or the In component is in the form of uniform gradient or gradient gradient in the middle layer 253 .

[0061] In one embodiment, the intermediate layer 253 may be composed of a GaN / InGaN superlattice structure, and the thickness of the intermediate layer 253 is between Alternatively, the stress release layer 250 may also be composed of a GaN / InGaN superlattice structure.

[0062] In one embodiment, the thickness of the middle layer 253 is greater than the thickness of the first sublayer 251, the thickness of the middle layer 253 is greater than the thickness of the second sublayer 252, and the thickness of the first sublayer 251 is less than the thickness of the second sublayer 252, thereby facilitating the release of stress. Between, for example, or The thickness of the second sub-layer 252 is between Between, for example, or The thickness of the intermediate layer 253 is between Between, for example, or

[0063] In one embodiment, an active layer 300 is formed on the first semiconductor layer, and the active layer 300 is located between the stress release layer 250 and the second waveguide layer 410. The active layer 300 can be set as a multilayer structure composed of nitride semiconductors such as GaN and InGaN. The active layer 300 has a single quantum well structure or a multiple quantum well structure. Compared with the single quantum well structure, the multiple quantum well structure is easier to obtain sufficient gain. In the case where the active layer 300 includes a multiple quantum well structure, if the well layer and the barrier layer are alternately stacked, the first and last layers can be either well layers or barrier layers. Further, the multiple quantum well structure includes 2 to 3 pairs of alternately arranged barrier layers and well layers, and the thickness of the second sublayer 252 of the stress release layer 250 is defined as H2, and the thickness of the first barrier layer close to the stress release layer 250 in the active layer 300 is L1, wherein 0.8≤H2 / L1≤1.2. That is, the thickness of the second sublayer 252 is similar to that of the first barrier layer, and the doping elements are similar. The second sublayer 252 is inserted between the intermediate layer 253 and the active layer 300 in the form of a pre-potential barrier layer to relieve stress between the active layer 300 and the first semiconductor layer. As an example, the thickness of the first barrier layer can be or The thickness of the second sub-layer 252 can also be or The thickness of the first sub-layer 251 is smaller than that of the second sub-layer 252 and the first barrier layer. For example, or In an optional implementation manner, the thickness of each barrier layer in the active layer 300 may be the same or different, and the thickness of each well layer may be the same or different.

[0064] Furthermore, for the semiconductor laser element emitting blue-green light, the active layer 300 in contact with the stress release layer 250 is the first well layer, and the first barrier layer, the second well layer and the second barrier layer are sequentially stacked from the first well layer upward. x Al y Ga 1-x-y N (0<x<1, 0≤y<1, 0<x+y<1), more preferably InGaN, the emission wavelength of the laser element can be controlled by adjusting the In content of the well layer to emit blue light or green light, and the emission wavelength range is 430nm~550nm.

[0065] Furthermore, for the semiconductor laser element emitting purple light, the active layer 300 in contact with the stress release layer 250 is the first well layer, and the first barrier layer, the second well layer, the second barrier layer, the third well layer and the third barrier layer are stacked in sequence from the first well layer upward. x Al y Ga 1-x-y N (0<x<1, 0≤y<1, 0<x+y<1), more preferably InGaN, the emission wavelength of the laser element can be controlled by adjusting the In content of the well layer to emit purple light, and the emission wavelength range is 370nm~450nm.

[0066] In one embodiment, a second semiconductor layer is formed on the active layer 300. The second semiconductor layer is a p-type semiconductor layer, which can be formed using a single layer or a multilayer structure formed of a nitride semiconductor layer. As the p-type nitride semiconductor layer contained in the second semiconductor layer, a layer formed of a nitride semiconductor containing p-type impurities such as Mg can be exemplified. The second semiconductor layer includes a second waveguide layer 410, an electron blocking layer 420, a second cladding layer 430, and an ohmic contact layer 440 stacked in sequence. The second semiconductor layer can also be configured with other layers in addition to the above layers, and a part of the layers can also be omitted.

[0067] In one embodiment, a second waveguide layer 410 is formed on the active layer 300, and its material may be InGaN. The addition of the In component can buffer the deformation of the well layer. The maximum content of the In component in the second waveguide layer 410 is greater than the peak intensity of the In component ion intensity curve L in the stress release layer 250, so as to achieve a good transition from the lattice constant of the active layer 300 to the second semiconductor layer. The thickness of the second waveguide layer 410 is similar to that of the first waveguide layer 240, both between 50nm and 500nm, so as to achieve a balance between the carrier injection efficiency, the refractive index and the layer structure strength. Further, the thickness of the second waveguide layer 410 is between 100nm and 300nm. In an optional embodiment, the In component in the second waveguide layer 410 gradually increases as it approaches the active layer 300, which can more effectively disperse the deformation of the well layer, improve the crystal quality of the active layer 300, and improve the carrier recombination efficiency.

[0068] In one embodiment, an electron blocking layer 420 is formed on the second waveguide layer 410, and its material can be a wide bandgap material such as AlN or AlGaN to effectively block the leakage of electrons from the second semiconductor layer to the active layer 300, while allowing holes to pass through. The second waveguide layer 410 and the electron blocking layer 420 work together in the laser to achieve the confinement of the light field and carriers, which helps to more effectively recombine the electrons and holes in the active region, thereby improving the light emission efficiency.

[0069] In one embodiment, a second cladding layer 430 is formed on the electron blocking layer 420. The material of the second cladding layer 430 may be a wide bandgap material such as AlGaN. The second cladding layer 430 limits the propagation of light in the waveguide layer by providing a lower refractive index than the second waveguide layer 410. The thickness of the second cladding layer 430 is between 100 nm and 500 nm to effectively limit the diffusion of carriers, while not being too thick to increase excessive series resistance.

[0070] In one embodiment, an ohmic contact layer 440 is formed on the second cladding layer 430. The material of the ohmic contact layer 440 may be GaN or InGaN, which matches the lattice constant of the second cladding layer 430. The electrical conductivity may be improved by high doping, thereby reducing the resistance of the contact with the metal electrode, forming a good ohmic contact, and promoting uniform injection of current.

[0071] In one embodiment of the present invention, the semiconductor laser element can form a ridge by etching part of the second semiconductor layer. The width of the ridge is adjusted to 1 μm to 5 μm. A contact electrode 500 is provided on the upper surface of the ridge. Specifically, the main function of the contact electrode 500 is to improve the lateral expansion capability and expand the area where the current acts. The material of the contact electrode 500 can be a transparent conductive film such as indium tin oxide (ITO), indium zinc oxide (IZO), zinc oxide (ZnO), gallium oxide (GaO3), etc. The material of the contact electrode 500 can also be a metal such as nickel and gold. The contact electrode 500 is a transparent conductive film having a refractive index smaller than that of the active layer 300. Further, an insulating layer 600 is formed on the side of the exposed ridge, the side of the contact electrode 500, and the surface of the second cladding layer 430 exposed by etching. The film thickness of the insulating layer 600 is between 100 nm and 500 nm, and it can be formed by a single layer or a multilayer film of materials such as oxides or nitrides of Si, Al, Zr, Ti, Nb, Ta, etc.

[0072] In one embodiment, the second electrode 700 is formed on the ridge and contacts the contact electrode 500 to be electrically connected to the second semiconductor layer. The thickness of the second electrode 700 is between 0.1 μm and 2 μm, and is generally sufficient to function as an electrode of a semiconductor laser element. The material of the second electrode 700 may be a metal or alloy such as Ni, Rh, Cr, Au, W, Pt, Ti, and Al.

[0073] In one embodiment, the first electrode 800 is disposed on the lower surface of the substrate 100 and is electrically connected to the first semiconductor layer. The material of the first electrode 800 includes any one or a combination of two or more of Ni, Ti, Pd, Pt, Au, Al, TiN, ITO, and IGZO, but is not limited thereto.

[0074] like Figure 3-4As shown, the relationship between the element concentration or ion intensity and depth in a partial range of a semiconductor laser element provided by an embodiment of the present application is shown. This relationship diagram can be obtained using a secondary ion mass spectrometer.

[0075] from Figure 3 It can be seen that the In component has an ion intensity curve L along the growth direction of the semiconductor stack, and the ion intensity curve L includes a first part S1, a second part S2, a third part S3 and a fourth part S4 connected in sequence; wherein, the ion intensity of the In component of the first part S1 gradually increases in the growth direction of the semiconductor and reaches a maximum value at the connection with the second part S2, the second part S2 includes a first trough T1, a second trough T2 and a middle section T3 located between the first trough T1 and the second trough T2, the ion intensity of the middle section T3 is greater than the ion intensity of the first trough T1 and the ion intensity of the second trough T2, the first trough T1 is connected to the first part S1, the second trough T2 is connected to the third part S3, the ion intensity of the In component of the third part S3 has two significant peaks, and the ion intensity of the In component of the fourth part S4 is the maximum value at the starting intensity at the connection with the third part S3 and gradually decreases along the growth direction of the semiconductor.

[0076] In the above embodiment, the ion intensity of the In component in the second part S2 is less than the maximum ion intensity of the In component in the first part S1, and the ion intensity of the In component in the middle section T3 is less than the maximum ion intensity of the fourth part S4, so as to avoid the carrier overflow phenomenon caused by the excessively high content of the In component in the middle section. Specifically, for the second part S2, the In ion intensity in the middle section T3 is greater than the In ion intensity in the first valley T1 and the second valley T2, and the semiconductor material corresponding to the middle section T3 can be, for example, InGaN, and the valleys on both sides contain a small amount of In component or no In component, and the semiconductor material corresponding to the valleys on both sides can be, for example, GaN. It can be understood that the signal duration of the In component ion intensity corresponds to the thickness of different semiconductor layers to a certain extent, and the layer thickness of the first part S1 is greater than the layer thickness corresponding to the second part S2; for the second part S2, the layer thickness of the middle section T3 is greater than the layer thickness corresponding to the first valley T1, and is also greater than the layer thickness corresponding to the second valley T1.

[0077] In this embodiment, the first waveguide layer 240 corresponds to Figure 1 The stress release layer 250 corresponds to the first portion S1 of the ion strength curve L, the active layer 300 corresponds to the third portion S3 of the ion strength curve L, and the second waveguide layer 410 corresponds to the fourth portion S4 of the ion strength curve L.

[0078] In one embodiment, the In component ion intensity of the stress release layer 250 is less than the maximum In ion intensity of the first waveguide layer 240 and the second waveguide layer 410, which reduces the lattice mismatch and reduces the structural defects. The lower In component content also means that the lattice constant of the layer is closer to the first well layer of the active layer 300, which is more conducive to achieving the stress release effect from the N-type semiconductor layer to the active layer 300. The thickness of the first waveguide layer 240 corresponding to the first part S1 is between 50nm and 500nm to achieve a balance between the electron injection efficiency, the refractive index and the layer structure strength. Further, the thickness of the first waveguide layer 240 is between 200nm and 400nm.

[0079] In one embodiment, the ratio of the In content of the stress release layer 250 corresponding to the second part S2 to the maximum value of the In content of the first waveguide layer 240 or the second waveguide layer 410 is between 1:8 and 1:4. The In content percentage of the first waveguide layer 240 and the second waveguide layer 410 is 4% to 8%, and the In content percentage of the second part S2, i.e., the stress release layer 250, is 0.5% to 2%. Further, the In content percentage of the stress release layer 250 is about 1%, and the In content in the stress release layer 250 preferably fluctuates within a range of 20% above and below 1%, and its lattice constant is between the first well layer in the active layer 300 and the substrate 100, achieving an effective lattice transition effect and good lattice matching, so that the interlayer stress can be released, the surface micropits of the active layer 300 are reduced, the interface flatness is improved, the crystal growth quality of the active layer 300 is improved, and the negative impact of the polarization field on the carrier recombination efficiency is reduced.

[0080] After testing, under the condition that other semiconductor layer parameters are the same, when the In content percentage in the active layer is 10% and the maximum In content percentages of the first waveguide layer 240 and the second waveguide layer 410 are both in the range of 4% to 8%, the sample with an In content of 8% in the stress release layer 250 is compared with the product with an In content of 1% in the stress release layer 250 provided in this embodiment. The light confinement capabilities of the two are basically the same, but the product with an In content of 1% has better active layer quality, smoother crystal surface growth, and improved product light brightness.

[0081] In an optional embodiment, the semiconductor layer corresponding to the middle section T3 of the second portion S2 is InGaN, and the semiconductor layers corresponding to the first valley T1 and the second valley T2 on both sides are GaN, that is, the In ion intensity curve of the second portion S2 is formed by a three-layer stacked structure of GaN / InGaN / GaN. Specifically, the middle section T3 corresponds to the middle layer 253 in the stress release layer 250, and the first valley T1 and the second valley T2 correspond to the first sublayer 251 and the second sublayer 252 in the stress release layer 250, respectively. The thickness of the first sublayer 251 is between between, preferably The thickness of the second sub-layer 252 is between between, preferably The thickness of the intermediate layer 253 is between between, preferably The overall thickness of the stress release layer 250 corresponding to the second portion S2 is between between, preferably In order to achieve a more balanced stress release effect. In an optional implementation, the intermediate layer 253 may be composed of a GaN / InGaN superlattice structure, or the stress release layer 250 may also be composed of a GaN / InGaN superlattice structure, which will not be described in detail here.

[0082] Furthermore, the semiconductor layer corresponding to the third part S3, that is, the In content percentage in the quantum well layer is between 10% and 15%. The In content in the stress release layer 250 should not be too high. When a higher content of In component is doped, for example, more than 2%, the stress release layer 250 plays a similar role to the well layer in the active layer 300 to a certain extent, which is easy to cause the overflow and recombination position shift of the carriers. The carriers originally recombined in the well layer shift toward the stress release layer 250, causing double peaks or multi-peak problems, the laser wavelength half-width becomes larger, the light shape becomes wider, and the light output brightness of the active layer 300 is lost. Similarly, the In content in the stress release layer 250 should not be too low. For example, if it is lower than 0.5%, it cannot play a good role in reducing the lattice mismatch, and it cannot effectively improve the surface flatness of the active layer 300.

[0083] It is understandable that for semiconductor lasers of other wavelengths, the emission wavelength can be adjusted by adjusting the In content in the active layer 300, thereby achieving light emission of different colors. Taking the green light semiconductor laser element as an example, the wavelength of green light is greater than the wavelength of blue light, and the In content in its active layer 300 is also relatively high. In order to confine the light between the waveguide layers, the difference in refractive index between the waveguide layer and the cladding layer should also be large, so the In content in the waveguide layer is also high relative to the blue light component, and the In content of the stress release layer of the green light component is also correspondingly high, so as to effectively achieve lattice constant matching between the first semiconductor layer and the active layer 300. For the green light semiconductor laser, the In ion intensity in the stress release layer 250 is also less than the In component content in the first waveguide layer 240 and the second waveguide layer 410. Furthermore, the stress release layer structure of the green semiconductor laser may also include a first sublayer 251, a second sublayer 252 stacked in sequence, and an intermediate layer 253 located between the first sublayer 251 and the second sublayer 252. The similarities with the above-mentioned structure and parameters of the blue semiconductor laser are not repeated here.

[0084] Continue to see Figure 3-4 , it can be seen that the Si element has a concentration curve n along the growth direction of the semiconductor stack, and the concentration curve n includes a first segment D1, a second segment D2 and a third segment D3 connected in sequence; wherein the first segment D1 corresponds to the area of ​​the first semiconductor layer away from the active layer 300, the third segment D3 corresponds to the area of ​​the first semiconductor layer close to the active layer 300, the concentration value of the second segment D2 is lower than the concentration value of the first segment D1, the Si element has a peak concentration in the third segment D3, and the concentration of the first segment D1 is greater than the peak concentration. The first segment D1 has a first concentration, the second segment D2 has a second concentration, and the third segment D3 has a peak concentration. The first concentration of the first segment D1 is greater than the peak concentration of the third segment D3, and the first concentration is between 8×10 18 atom / cm 3 ~1.5×10 19 atom / cm 3 , which can effectively increase the electron injection efficiency and improve the quantum efficiency of the laser.

[0085] In one embodiment, the peak concentration of the third segment D3 is less than or equal to 1.2×10 19 atom / cm 3 The third segment D3 is a semiconductor layer close to the active layer 300. Limiting its peak concentration can avoid defects in the crystal caused by excessive doping concentration and reduce the polarization electric field phenomenon in the stress release layer 250. It can be understood that by optimizing the distribution of Si elements, the third segment D3 may have more than one peak concentration to optimize the performance of the semiconductor laser element. In an optional embodiment, when the third segment D3 corresponds to a multiple stacked structure composed of different materials, such as a GaN / InGaN / GaN multilayer structure, the doping peak concentration can be generated in any semiconductor sublayer corresponding to the third segment D3, and the first concentration of the first segment D1 is greater than the highest peak concentration of the third segment D3.

[0086] In this embodiment, the electron supply layer 230 corresponds to Figure 2 The first waveguide layer 240 corresponds to the first segment D1 of the concentration curve n, the first waveguide layer 240 corresponds to the second segment D2 of the concentration curve n, and the stress release layer 250 corresponds to the third segment D3 of the concentration curve n.

[0087] In the above embodiment, the first segment D1 may be AlGaN material with a high Si doping concentration greater than 3×10 18 atom / cm 3 Specifically, the doping concentration is between 3×10 18 atom / cm 3 ~1.5×10 19 atom / cm 3By inserting a highly doped first segment D1 before the second segment D2, sufficient electron concentration is provided to improve the electron-hole recombination efficiency and thus enhance the luminous brightness. Furthermore, the doping concentration of the first segment D1 is between 1×10 19 atom / cm 3 ~1.2×10 19 atom / cm 3 The concentration of the second segment D2 is between 5×10 17 atom / cm 3 ~5×10 18 atom / cm 3 The peak concentration of the third segment D3 is between 1×10 18 atom / cm 3 ~5×10 19 atom / cm 3 , but less than the doping concentration of the first section D1, the stress release layer 250 corresponding to the third section D3 is relatively highly doped to reduce the influence of the polarization field on the carrier recombination efficiency in the active layer 300, and further, the peak concentration of the third section D3 is less than or equal to 1.2×10 19 atom / cm 3 .

[0088] In one embodiment, the third section D3, i.e., the stress release layer 250, is relatively highly doped to suppress the polarization field to improve the carrier recombination efficiency, such as Si doping. However, the highly doped semiconductor layer will cause serious light absorption, reduce the gain effect, and cause the performance of the semiconductor laser element to decline. Therefore, the thickness of the stress release layer 250 should not be too large. It can be understood that the duration of the Si concentration signal corresponds to the thickness of different semiconductor layers to a certain extent. The thickness of the third section D3, i.e., the stress release layer 250, is Preferably, further, the thickness of the stress release layer 250 is between

[0089] In the above embodiment, the Si concentration of the semiconductor layer corresponding to the first section D1, i.e., the electron supply layer 230, is greater than the peak concentration in the third section D3, i.e., the stress release layer 250, and the Si element is uniformly doped along the growth direction of the semiconductor stack, and the initial doping concentration from the lower surface to the doping concentration on the upper surface is always consistent. The constant doping concentration is conducive to simplifying the preparation process, and also keeps the electron concentration in the electron supply layer 230 stable, which can improve the performance stability of the semiconductor laser element. The insertion of the electron supply layer 230 can optimize the number and distribution of carriers in the active layer 300 and improve the quantum efficiency of the laser. The doping concentration in the layer is between 8×10 18 atom / cm 3 ~1.5×10 19atom / cm 3 In order to provide enough electrons to the quantum well layer for effective recombination. In an optional embodiment, the doping concentration of the first segment D1 can also be uniformly graded doping or gradient graded doping.

[0090] In one embodiment, the thickness of the electron supply layer 230 is less than the thickness of the first waveguide layer 240. The relatively thin electron supply layer 230 can reduce the defects caused by the crystal growth in the layer, ensure a higher gain coefficient, and provide a relatively flat surface as the growth basis of the first waveguide layer 240, which is conducive to improving the crystal quality of the first waveguide layer 240. The thickness of the electron supply layer 230 is 10nm to 50nm. Further, the thickness of the electron supply layer 230 is between 15nm and 25nm, for example, 20nm, to achieve a good balance between the electron supply capability and the quality of the layer structure.

[0091] This embodiment further provides a light-emitting device, which includes any one of the semiconductor laser elements in the above embodiments, so the light-emitting device also has the above excellent effects.

[0092] In summary, the semiconductor laser element and light-emitting device provided by the present application effectively overcome various shortcomings in the prior art and have high industrial utilization value.

[0093] The above embodiments are merely illustrative of the principles and effects of the present application and are not intended to limit the present application. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present application shall still be covered by the claims of the present application.

Claims

1. A semiconductor laser element, It is characterized in that At least: A semiconductor stack, wherein the semiconductor stack comprises a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence; The first semiconductor layer includes a first waveguide layer, the second semiconductor layer includes a second waveguide layer, and the first waveguide layer and the second waveguide layer are both located on a side of the corresponding semiconductor layer close to the active layer; wherein, A stress release layer is also included between the first waveguide layer and the active layer, at least part of the stress release layer contains an In component, and the In component forms an ion intensity curve along the growth direction of the semiconductor stack. The peak intensity of the In component in the stress release layer in the ion intensity curve is less than the maximum content of the In component in the first waveguide layer.

2. The semiconductor laser element according to claim 1, It is characterized in that The peak intensity of the ion intensity curve of the In component of the stress release layer is less than the In component content in the second waveguide layer.

3. The semiconductor laser element according to claim 1, It is characterized in that The ion strength curve of the stress release layer has a first valley, a second valley, and a middle section between the first valley and the second valley, wherein: The In component ion intensity of the middle segment is less than the In component content in the first waveguide layer and / or the second waveguide layer.

4. The semiconductor laser element according to claim 1, It is characterized in that The stress release layer includes a first sublayer, a second sublayer and an intermediate layer located between the first sublayer and the second sublayer, wherein the first sublayer and the second sublayer include GaN, and the intermediate layer contains an In component and has an intensity peak of an ion intensity curve of the In component.

5. A semiconductor laser element, It is characterized in that At least: A semiconductor stack, wherein the semiconductor stack comprises a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence; The first semiconductor layer includes a first waveguide layer, the second semiconductor layer includes a second waveguide layer, and the first waveguide layer and the second waveguide layer are both located on a side of the corresponding semiconductor layer close to the active layer; wherein, A stress release layer is further included between the first waveguide layer and the active layer, wherein the stress release layer includes a first sublayer, a second sublayer and an intermediate layer located between the first sublayer and the second sublayer, the intermediate layer contains an In component, and the thickness of the intermediate layer is between The thickness of the stress release layer is between between.

6. The semiconductor laser element according to claim 4 or 5, It is characterized in that The first sublayer and the second sublayer include GaN; and the intermediate layer includes InGaN.

7. The semiconductor laser element according to claim 4 or 5, It is characterized in that The thickness of the intermediate layer is greater than the thickness of the first sub-layer or the second sub-layer.

8. The semiconductor laser element according to claim 4 or 5, It is characterized in that The thickness of the first sublayer is between The thickness of the second sublayer is between between.

9. The semiconductor laser element according to claim 4 or 5, It is characterized in that The In component content of the intermediate layer is between 0.5% and 2.0%.

10. The semiconductor laser element according to claim 4 or 5, It is characterized in that The In component content percentage of the first waveguide layer is between 4.0% and 8.0%.

11. The semiconductor laser element according to claim 4 or 5, It is characterized in that The ratio of the In content of the intermediate layer to the maximum value of the In content of the first waveguide layer or the second waveguide layer is between 1:8 and 1:

4.

12. The semiconductor laser element according to claim 4 or 5, It is characterized in that The active layer is a multiple quantum well structure, which includes 2 to 3 pairs of barrier layers and potential well layers arranged alternately; the thickness of the second sublayer is H 2 , the thickness of the barrier layer close to the second sublayer is L 1 , where 0.8≤H 2 :L 1 ≤1.

2.

13. The semiconductor laser element according to claim 1 or 5, It is characterized in that The first semiconductor layer further includes a first cladding layer and an electron supply layer, and the electron supply layer is located between the first cladding layer and the first waveguide layer.

14. The semiconductor laser element according to claim 13, It is characterized in that The thickness of the electron supply layer is less than or equal to 100 nm.

15. The semiconductor laser element according to claim 1 or 5, It is characterized in that The light emission wavelength of the laser element is 430nm-550nm.

16. A light emitting device, It is characterized in that The light emitting device includes the semiconductor laser element according to any one of claims 1 to 15.

Citation Information

Patent Citations

  • Short wavelength AlGaInP red light semiconductor laser

    CN105390937A

  • Semiconductor device, semiconductor laser, and high electron mobility transistor

    CN1153411A

  • Semiconductor laser with light field loss control layer

    CN116316065A

  • Semiconductor laser

    CN116914564A

  • Semiconductor luminous element and its manufacture

    JP2000332363A