Semiconductor single-walled carbon nanotube parallel array and preparation method and application thereof
By using carbon monoxide and bimetallic catalysts to grow semiconductor single-walled carbon nanotubes under high temperature conditions, the complexity and energy consumption of the preparation of high-purity carbon nanotube arrays in the prior art are solved, and high efficiency and green carbon is achieved Nanotube preparation, suitable for high-performance construction of field effect transistor devices.
Patent Information
- Application Number
- CN202310625834.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to effectively prepare high-purity semiconductor single-wall carbon nanotube parallel arrays, especially while maintaining high density and consistent orientation of materials, the process is complex and energy-consuming, which limits the large-scale application of carbon-based nano electronic devices. .
Using carbon monoxide as the carbon source, a parallel array of semiconductor single-walled carbon nanotubes is grown on a flat substrate under high temperature conditions. The metallic carbon nanotubes are selectively etched through carbon dioxide generated in situ by carbon monoxide dismutation reaction. Achieve high purity semiconductor tube enrichment.
The preparation of semiconductor single-wall carbon nanotube parallel arrays with high purity (up to 97%) is achieved, which simplifies the process flow, reduces energy consumption, and supports the green, efficient and large-scale preparation of carbon nanotubes to meet the needs of High performance requirements for field effect transistor devices.
Smart Images

Figure HDA0004257097340000011 
Figure HDA0004257097340000012 
Figure HDA0004257097340000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of carbon nanotubes, and in particular relates to a semiconductor single-wall carbon nanotube parallel array and a preparation method thereof, as well as an application of the semiconductor single-wall carbon nanotube parallel array in a field effect transistor device. Background Art
[0002] Single-walled carbon nanotubes (SWCNTs) have unique quasi-one-dimensional structures and excellent electrical, thermal and mechanical properties, and have shown broad application prospects in the fields of nanoelectronic devices, sensors, bioimaging, energy and environment. Among them, semiconducting single-walled carbon nanotubes have outstanding physical and electronic properties such as small size, high carrier mobility, no dangling bonds on the surface, and adjustable band gap. They have shown great advantages of both high performance and low power consumption in field effect transistor (FET) devices and complementary metal oxide semiconductor (CMOS) integrated circuits, becoming one of the most promising new semiconductor materials. High-performance carbon nanotube-based devices require materials with high semiconducting tube purity, high density and highly consistent orientation. Therefore, the controllable preparation of parallel arrays of single-walled carbon nanotubes, especially the improvement of the semiconducting tube purity of parallel arrays, is of great significance for the large-scale application of carbon-based nanoelectronic devices. However, metallic tubes and semiconducting tubes usually coexist in single-walled carbon nanotube samples, making the preparation of high-purity semiconducting single-walled carbon nanotube parallel arrays extremely challenging.
[0003] At present, there are two main strategies for preparing parallel arrays of semiconducting single-walled carbon nanotubes on substrates: solution assembly and direct growth by chemical vapor deposition. The method of directional assembly of carbon nanotube dispersion can obtain a high-density carbon nanotube array, but this method requires multiple ultrasonic dispersions, which causes the carbon nanotubes to be shortened, introduces defects, and has residual dispersant that is difficult to remove, limiting the improvement of device performance. Compared with the solution method, the single-walled carbon nanotube parallel arrays grown directly by chemical vapor deposition have highly consistent orientation, suitable and adjustable length, and clean surface, which is convenient for direct use in the construction and integration of devices such as field effect transistors, and can greatly shorten the process flow.
[0004] Metallic tubes have a continuous density of states near the Fermi level, while semiconducting tubes have a band gap at the Fermi level, so the chemical reactivity of metallic tubes is higher than that of semiconducting tubes. Therefore, the difference in chemical activity between metallic tubes and semiconducting tubes is often used to selectively etch metallic tubes or inhibit their nucleation by adjusting the growth atmosphere to achieve the selective growth of semiconducting tubes. Studies have found that the additional introduction of etching gases such as H2O or the use of free radicals generated by carbon source cracking (such as hydroxyl radicals generated by methanol cracking) can effectively remove metallic tubes, and up to about 97% of semiconducting tube enrichment can be obtained. It is worth noting that in almost all literature reports on the growth of parallel arrays of semiconducting single-walled carbon nanotubes, the reaction gas is composed of two or more components. The complex growth atmosphere makes the growth regulation of carbon nanotubes more complicated, and the growth conditions of high selectivity are also more demanding. In addition, hydrogen is often required to be introduced into the carbon source gas as a regulator, and the use of high-flow hydrogen will cause a lot of energy waste. Therefore, in addition to highly selective growth, the current research focus of single-walled carbon nanotube parallel arrays should also focus on developing preparation methods that are simple in process, green in process, and easy to scale up, so as to achieve large-scale and controllable preparation of single-walled carbon nanotube parallel arrays for device applications.
[0005] Carbon monoxide (CO) is widely available in industrial production and is often obtained through the water-gas reaction. It is the first carbon source gas used to prepare high-quality commercial bulk single-walled carbon nanotubes. The process is usually carried out under high pressure. CO molecules undergo a disproportionation reaction to generate carbon for the growth of carbon nanotubes: The reaction is simple, and almost no other side reactions occur. Therefore, the gas phase composition of the reaction system is simple, with only two gases, CO and CO2, which can create a relatively simple reaction environment, making the growth of carbon nanotubes easier to control. In addition, the CO2 produced by the reaction is weakly oxidizing, and may also play a certain regulatory role in the growth of carbon nanotubes. If the small amount of CO2 produced can be removed by a gas adsorption device, it is also possible to achieve the recycling of carbon source gas, which is difficult to achieve with other hydrogen-containing carbon sources. In addition, CO is commonly used in industrial metal refining, so it may be used as a reducing agent to prepare catalyst nanoparticles. Some reports have found that using CO as a carbon source is beneficial for the preparation of bulk single-walled carbon nanotube samples enriched with small-diameter semiconductor tubes, but there are few reports on selective growth on a flat substrate, especially the selective preparation of parallel arrays of single-walled carbon nanotubes.
[0006] In summary, the development of a simple, green, efficient and scalable method for preparing parallel arrays of semiconducting single-walled carbon nanotubes is of great significance for the industrial application of carbon-based nanoelectronic devices, and will also help promote continuous progress in the field of carbon nanotube research. Summary of the invention
[0007] To solve the above problems, the present invention provides a parallel array of semiconducting single-walled carbon nanotubes. Using carbon monoxide as a carbon source and a bimetallic catalyst, a parallel array of semiconducting single-walled carbon nanotubes is selectively grown on a flat substrate. It has a narrow diameter distribution, which is conducive to the selective etching of metallic carbon nanotubes by carbon dioxide generated in situ by the carbon monoxide disproportionation reaction, thereby obtaining high-purity semiconducting single-walled carbon nanotubes. Semiconducting enrichment can be obtained in a wider growth window and a variety of bimetallic catalyst systems. In the above growth process, CO gas is used as a reducing gas and a carbon source at the same time, and there is no need to introduce any other gas. In the future, it is expected to develop a large-scale preparation method for semiconducting single-walled carbon nanotubes on this basis.
[0008] The object of the present invention is to provide a semiconductor single-walled carbon nanotube parallel array, wherein the semiconductor tube content is greater than 90%, preferably greater than 93%, more preferably greater than 95%, such as 97%.
[0009] The present invention also aims to provide a method for preparing a semiconductor single-walled carbon nanotube parallel array, which is grown on a substrate in the presence of a bimetallic catalyst, in a carbon monoxide atmosphere, and under high temperature conditions.
[0010] The method specifically comprises the following steps:
[0011] Step 1. Arrange and prepare bimetallic oxides on a substrate to obtain a substrate loaded with bimetallic oxides;
[0012] Step 2. placing the substrate loaded with the bimetallic oxide in a protective atmosphere and heating it to a growth temperature;
[0013] Step 3: Continue to introduce carbon monoxide to grow and obtain a parallel array of semiconducting single-walled carbon nanotubes.
[0014] Another object of the present invention is to provide a use of the semiconductor single-walled carbon nanotube parallel array, which is used as a channel material to prepare a field effect transistor device.
[0015] Another object of the present invention is to provide a field effect transistor device, the channel of which is constructed by the parallel array of semiconducting single-walled carbon nanotubes.
[0016] The semiconductor single-walled carbon nanotube parallel array and the preparation method thereof provided by the present invention have the following beneficial effects:
[0017] (1) The semiconducting single-walled carbon nanotube parallel array of the present invention has a high purity of semiconducting tubes, which can reach up to 97%, and can meet the requirements of field effect transistor devices for high semiconducting tube purity and highly consistent orientation.
[0018] (2) The field effect transistor device constructed by using the parallel array of semiconducting single-walled carbon nanotubes in the present invention as a channel can obtain a semiconducting field effect transistor device with an extremely high switching ratio.
[0019] (3) The method for preparing the parallel array of semiconducting single-walled carbon nanotubes in the present invention is simple to operate and easy to control and implement.
[0020] (4) The method of the present invention is applicable to a variety of catalyst systems and has a wide growth temperature window.
[0021] (5) The method of the present invention only introduces carbon monoxide as both a reducing gas and a carbon source, and the gas composition is simple, which facilitates the recycling of the carbon source gas, and is expected to achieve green, efficient, and large-scale preparation of carbon nanotubes for device applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The SEM image of the semiconductor single-walled carbon nanotube parallel array prepared in Example 1 of the present invention is shown;
[0023] Figure 2 The mapping Raman spectrum of the semiconductor single-walled carbon nanotube parallel array prepared in Example 1 of the present invention is obtained by testing at an excitation wavelength of 532 nm;
[0024] Figure 3 The mapping Raman spectrum of the semiconductor single-walled carbon nanotube parallel array prepared in Example 1 of the present invention is obtained by testing at an excitation wavelength of 633 nm;
[0025] Figure 4 The mapping Raman spectrum of the semiconductor single-walled carbon nanotube parallel array prepared in Example 1 of the present invention is obtained by testing at an excitation wavelength of 785 nm;
[0026] Figure 5 The typical transfer characteristic curve of the effect transistor device constructed by the parallel array of semiconducting single-walled carbon nanotubes prepared in Example 1 of the present invention is shown. DETAILED DESCRIPTION
[0027] The present invention is described in detail below through specific implementation modes, and the characteristics and advantages of the present invention will become clearer and more specific with these descriptions.
[0028] The present invention provides a parallel array of semiconducting single-walled carbon nanotubes, wherein the proportion of the number of semiconducting tubes is greater than 90%, preferably greater than 93%, more preferably greater than 95%, such as 97%.
[0029] The invention provides a method for preparing a semiconductor single-wall carbon nanotube parallel array, which is grown on a substrate in the presence of a bimetallic catalyst, in a carbon monoxide atmosphere and under high temperature conditions.
[0030] The method specifically comprises the following steps:
[0031] Step 1. Arrange and prepare bimetallic oxides on a substrate to obtain a substrate loaded with bimetallic oxides.
[0032] In step 1, a bimetallic catalyst precursor solution is coated on a pretreated substrate, and then oxidized under high temperature and in an oxygen atmosphere to obtain a substrate loaded with bimetallic oxides.
[0033] The bimetallic catalyst precursor solution is obtained by adding a first metal compound and a second metal compound into a solvent, followed by dissolving or dispersing the mixture.
[0034] The metal elements in the bimetallic catalyst are selected from two of the third period metal elements, transition metal elements except actinides, potassium elements and calcium elements, such as sodium (Na), magnesium (Mg), aluminum (Al), potassium (K), calcium (Ca), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt), gold (Au), lead (Pb) and lanthanide elements, preferably two of iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), manganese (Mn), molybdenum (Mo) and tungsten (W) elements, and more preferably bimetallic elements of cobalt (Co) and copper (Cu).
[0035] The solvent is selected from one or more of water, alcohol solvents, ether solvents, ketone solvents, aromatic hydrocarbon solvents, alkane solvents and halogenated hydrocarbon solvents, preferably one or more of water, methanol, ethanol, propanol, isopropanol, methyl ether, ethyl ether, methyl ethyl ether, acetone, benzene, toluene, xylene, hexane, carbon tetrachloride, chloroform and dichloromethane, more preferably one or more of water, methanol, ethanol, isopropanol and toluene, such as anhydrous ethanol.
[0036] In the bimetallic catalyst precursor solution, the concentration of the first metal compound or the second metal compound is 0.01 to 1000 mmol / L, preferably 0.5 to 20 mmol / L, more preferably 1 to 10 mmol / L, such as 1 to 3 mmol / L. The concentrations of the first metal compound and the second metal compound will affect the size and density of the bimetallic catalyst nanoparticles prepared subsequently, and further affect the growth of carbon nanotubes. Too high or too low concentrations of the first metal compound and the second metal compound will result in a lower density of the grown single-walled carbon nanotube parallel array.
[0037] The pretreatment is to perform annealing and hydrophilic treatment on the substrate in sequence. Annealing is to place the substrate at 850-1050°C for 0.5-1h to clean impurities on the substrate surface and repair lattice defects to make the growth substrate smoother. Hydrophilic treatment is to perform hydrophilic treatment on the annealed substrate using air plasma.
[0038] The oxidation treatment temperature is 300-800°C, preferably 350-700°C, more preferably 400-600°C, such as 450°C. The treatment time is 1-100 min, preferably 2-20 min, more preferably 5-10 min. The oxygen atmosphere is an air atmosphere or an oxygen atmosphere, preferably an air atmosphere. After the oxidation treatment, the first metal compound and the second metal compound are converted into oxides.
[0039] Step 2: Place the bimetallic oxide loaded substrate in a protective atmosphere and heat it to the growth temperature.
[0040] The growth temperature is 500-1200°C, preferably 650-1000°C, more preferably 850-950°C, such as 950°C. The protective atmosphere is a nitrogen atmosphere or an argon atmosphere, preferably an argon atmosphere. The present invention has found through a large number of experiments that as the growth temperature increases, the average diameter of the grown single-walled carbon nanotubes increases. This is because the growth temperature affects the cracking of the carbon source and the activity and state of the catalyst. Only at a suitable temperature, the grown carbon nanotubes have a suitable tube diameter and a narrow diameter distribution, which is conducive to the selective etching of the metallic tubes by the CO2 produced by the CO disproportionation reaction, thereby realizing semiconductor selective growth. In particular, when the growth temperature is 850-950°C, the semiconductor tube content of the grown parallel array is higher than 90%, and can reach up to 97% or more.
[0041] Step 3: Continue to introduce carbon monoxide to grow and obtain a parallel array of semiconducting single-walled carbon nanotubes.
[0042] Continue to introduce carbon monoxide, and stop introducing argon. The carbon monoxide flow rate is 10-1000cm 3 / min, preferably 50 to 200 cm 3 / min, more preferably 80 to 120 cm 3 / min, such as 100cm 3 / min. The experiment found that the carbon monoxide flow rate affects the semiconductor selectivity of the single-walled carbon nanotube parallel array. When the carbon monoxide flow rate is low, the gas stays in the heating zone for a longer time and is fully heated to promote the forward disproportionation reaction. However, when the carbon monoxide flow rate is lower than 10cm 3 / min, too low a flow rate is not conducive to the timely removal of CO2 gas, which may lead to an enhanced etching effect on carbon nanotubes; when the carbon monoxide flow rate is high, the gas is not fully heated, resulting in less CO2 production, and the flow rate above 1000cm 3 / min results in a weaker etching effect on metallic tubes and a decrease in the purity of the semiconductor tubes in the final product.
[0043] The growth time is 1 to 600 min, preferably 5 to 60 min, and more preferably 10 to 20 min.
[0044] The invention also provides the use of the semiconductor single-wall carbon nanotube parallel array, which is used as a channel material to prepare a field effect transistor device.
[0045] The invention also provides a field effect transistor device, the channel of which is constructed by the semiconductor single-wall carbon nanotube parallel array.
[0046] The switching ratio of the field effect transistor device is 10 4 ~10 8 , preferably 10 6 ~10 8 , more preferably 10 8 .
[0047] The present invention uses a bimetallic catalyst for catalysis and carbon monoxide as a carbon source to prepare a semiconductor single-walled carbon nanotube parallel array with high-purity semiconductor tubes. The semiconductor tubes have high purity and good orientation. The semiconductor field effect transistor device can be stably constructed as a channel material. The obtained field effect transistor device has an extremely high switching ratio, thereby meeting people's use needs.
[0048] Example
[0049] Example 1
[0050] 0.01 g of cobalt acetate tetrahydrate (about 0.04 mmol) and 0.008 g (about 0.04 mmol) of copper acetate monohydrate were dissolved in 20 mL of anhydrous ethanol to obtain a bimetallic catalyst precursor solution with a Co and Cu concentration of about 2 mM, wherein the molar ratio of Co to Cu was about 1:1.
[0051] The clean ST-cut quartz wafer was first annealed in air at 950°C for 0.5 h to clean the impurities on the substrate surface and repair the lattice defects to make the growth substrate smoother, and then it was hydrophilized using air plasma.
[0052] The catalyst precursor solution was spin-coated on the hydrophilic quartz substrate, and then the quartz substrate loaded with the catalyst precursor was placed on a slide and placed in a quartz tube, and pushed to the edge of the heating zone of the tube furnace. When the temperature rises to 450°C, the slide loaded with the quartz substrate was pushed to the center of the constant temperature zone of the tube furnace and oxidized in air for 5 minutes.
[0053] The quartz tube was sealed and argon was introduced to exhaust the gas inside. When the growth temperature rose to 925°C, the argon was stopped and the temperature was 100 cm 3 / min flow rate, carbon monoxide was introduced for 20min growth, and after the growth was completed, the temperature was naturally cooled to room temperature under the protection of argon and then taken out. Thus, a semiconductor single-walled carbon nanotube parallel array was prepared on the quartz substrate, and its scanning electron microscope SEM image is shown as follows Figure 1 As shown. Figure 1 It can be seen that the obtained semiconducting single-walled carbon nanotube parallel array is well arranged, has consistent orientation and a clean surface.
[0054] Example 2
[0055] A semiconductor single-walled carbon nanotube parallel array was obtained according to the method of Example 1, except that the growth temperature was 850°C.
[0056] Example 3
[0057] Semiconducting single-walled carbon nanotube parallel arrays were prepared according to the method of Example 1, except that manganese acetate was used instead of copper acetate monohydrate to prepare a bimetallic catalyst precursor solution with Co and Mn concentrations of about 2 mM; and the growth temperature was 900°C.
[0058] Experimental example
[0059] Experimental Example 1
[0060] The semiconductor single-walled carbon nanotube parallel array grown on the quartz substrate in Example 1 is transferred to the SiO2 / Si substrate. For the specific method, see the document Nano Research 2014, 7(7), 981-989.
[0061] The Raman spectrum test of the above semiconductor single-walled carbon nanotube parallel array was carried out, the excitation wavelengths were 532, 633 and 785nm respectively, the mapping method was surface scanning, and the test results were as follows: Figure 2 , Figure 3 , Figure 4As shown, according to the Kataura diagram, the semiconductor tube and metallic tube regions can be identified, corresponding to the S and M regions in the figure respectively.
[0062] It can be seen that the carbon nanotubes excited by 532nm laser are all semiconductor tubes ( Figure 2 ), the majority of carbon nanotubes excited by 633nm laser are semiconducting tubes ( Figure 3 ), 785nm laser hardly stimulates carbon nanotubes ( Figure 4 ). According to statistics, the grown semiconducting single-walled carbon nanotube parallel arrays exhibited high semiconductor selectivity, with a semiconducting tube content of about 97%.
[0063] According to the above method, the content of semiconductor tubes in the single-walled carbon nanotube parallel array obtained in Example 2 is about 92%.
[0064] According to the above method, the content of semiconductor tubes in the semiconductor single-walled carbon nanotube parallel array obtained in Example 3 is about 93%.
[0065] Experimental Example 2
[0066] The single-walled carbon nanotube parallel array grown in Example 1 was transferred to a SiO2 / Si substrate to construct a back-gate field effect transistor device for electrical measurement. The typical transfer characteristic curve of the device was tested, such as Figure 5 shown.
[0067] The single-walled carbon nanotube parallel array grown on a quartz substrate was transferred to a labeled SiO2 / Si substrate; Ti (0.5nm) / Pd (20nm) / Au (20nm) was deposited by electron beam evaporation, and the source and drain contact electrodes were formed by peeling to construct a back-gate FET device; the carbon nanotubes around the device were removed by a reactive ion etching system to obtain a field effect transistor device. The electrical measurement results of the field effect transistor device were obtained using a semiconductor characterization system (Keithley 4200).
[0068] from Figure 5 As can be seen from the figure, the device has an extremely high on / off ratio, up to 10 8 , that is, there are no metallic tubes in the array. The inset is a scanning electron microscope image of the constructed device. The electrical measurement results of 40 carbon nanotube devices can be calculated to show that the content of semiconductor tubes in the sample is as high as 97%. The above results are consistent with the Raman characterization results, further indicating the enrichment of semiconductor tubes in the prepared single-walled carbon nanotube parallel array sample.
[0069] The present invention is described in detail above in conjunction with specific embodiments and / or exemplary examples and drawings, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, various equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
Claims
1. A parallel array of semiconducting single-walled carbon nanotubes, wherein: The proportion of semiconductor tubes is greater than 90%, preferably greater than 93%, and more preferably greater than 95%.
2. A method for preparing a parallel array of semiconducting single-walled carbon nanotubes, characterized in that: The nanostructured carbon monoxide is grown on a substrate in the presence of a bimetallic catalyst, in a carbon monoxide atmosphere and under high temperature conditions.
3. The preparation method according to claim 2, characterized in that: The method specifically comprises the following steps: Step 1. Arrange and prepare bimetallic oxides on a substrate to obtain a substrate loaded with bimetallic oxides; Step 2. placing the substrate loaded with the bimetallic oxide in a protective atmosphere and heating it to a growth temperature; Step 3: Continue to introduce carbon monoxide to grow and obtain a parallel array of semiconducting single-walled carbon nanotubes.
4. The preparation method according to claim 3, characterized in that: In step 1, a bimetallic catalyst precursor solution is coated on a pretreated substrate, and then oxidized under high temperature and in an oxygen atmosphere to obtain a substrate loaded with bimetallic oxides.
5. The preparation method according to claim 4, characterized in that: In step 1, in the bimetallic catalyst precursor solution, the concentration of the first metal compound or the second metal compound is 0.01 to 1000 mmol / L, preferably 0.5 to 20 mmol / L, and more preferably 1 to 10 mmol / L.
6. The preparation method according to claim 2, characterized in that: The metal elements in the bimetallic catalyst are selected from two of the third period metal elements, transition metal elements except actinides, potassium elements and calcium elements, such as sodium (Na), magnesium (Mg), aluminum (Al), potassium (K), calcium (Ca), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt), gold (Au), lead (Pb) and lanthanide elements, preferably two of iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), manganese (Mn), molybdenum (Mo) and tungsten (W) elements, and more preferably bimetallic elements of cobalt (Co) and copper (Cu).
7. The preparation method according to claim 4, characterized in that: The oxidation treatment temperature is 300-800°C, preferably 350-700°C, more preferably 400-600°C; the treatment time is 1-100 min, preferably 2-20 min, more preferably 5-10 min.
8. The preparation method according to claim 3, characterized in that: In step 2, the growth temperature is 500-1200°C, preferably 650-1000°C, and more preferably 850-950°C.
9. The preparation method according to claim 3, characterized in that: In step 3, the carbon monoxide flow rate is 10 to 1000 cm 3 / min, preferably 50 to 200 cm 3 / min, more preferably 80 to 120 cm 3 / min, The growth time is 1 to 600 min, preferably 5 to 60 min, and more preferably 10 to 20 min.
10. A field effect transistor device, characterized in that: The field effect transistor device channel is constructed by a parallel array of semiconducting single-walled carbon nanotubes according to claim 1, The switching ratio of the field effect transistor device is 10 4 ~10 8 , preferably 10 6 ~10 8 , more preferably 10 8 .