Diffusion barrier coating with corrosion and contaminant protection

By forming a multi-layer corrosion-resistant coating on the metal components of the semiconductor processing system, including oxygen-containing materials and barrier layers, the problems of corrosion and pollutant diffusion are solved, and the corrosion resistance and stability of the equipment are improved.

CN119072559APending Publication Date: 2024-12-03APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035942.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-05
Filing Date
2023-03-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Metal components in semiconductor processing systems are prone to corrosion in high temperature, low temperature, high pressure and corrosive environments, resulting in equipment wear and pollutants. The prior art is difficult to effectively prevent corrosion and the diffusion of pollutants.

Method used

Using a multi-layer corrosion-resistant coating, including forming a first oxygen-containing material and a second oxygen-containing material on the substrate, and forming a barrier layer therebetween, the barrier layer may be less than or about 25 nm, and by deposition of atomic layer to form an alternating stack To enhance corrosion resistance and expose the substrate to halogen-containing species to reduce corrosion and contaminants movement.

Benefits of technology

It significantly improves the resistance of metal components to highly corrosive environments, extends the operating life of the equipment, reduces the generation and propagation of pollutants, and improves the stability and efficiency of semiconductor processing systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072559A_ABST
    Figure CN119072559A_ABST
Patent Text Reader

Abstract

Example methods of semiconductor processing are described. This method has been developed to increase corrosion resistance of substrates, such as metal substrates. The method includes forming a first oxygen-containing material on a substrate. The first oxygen-containing material may be or include silicon oxide, yttrium oxide, or aluminum oxide. The method may include forming a barrier layer on a first oxygen-containing material. The method may include forming a second oxygen-containing material on the barrier layer. The second oxygen-containing material may be or include silicon oxide, yttrium oxide, or aluminum oxide.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority to U.S. Patent Application No. 17 / 713,350, filed on April 5, 2022, entitled “COATINGS WITH DIFFUSION BARRIERS FOR CORROSION AND CONTAMINATION PROTECTION,” which is hereby incorporated by reference in its entirety. Technical Field

[0003] The present technology relates to processes and systems for coating parts. More specifically, the present technology relates to systems and methods for coating substrates with multi-layer anti-corrosion and anti-fouling coatings. Background Art

[0004] Semiconductor processing systems may include several components for supporting substrates, delivering formation materials and removing materials, and defining processing areas and flow paths. These components may be exposed to high and low temperatures, high and low pressures, and various corrosive and erosive materials. Therefore, many processing chambers include treated or coated materials. However, as processing systems and chambers become more complex, the components incorporated into the system may become multi-piece devices that may include complex geometries and features throughout the component. These features may similarly be exposed to environmental conditions and materials that may cause damage to the component.

[0005] Therefore, there is a need for improved systems and components that can be used to produce high quality devices and structures. These needs and other needs are met by the present technology. Summary of the invention

[0006] Embodiments of the present technology include semiconductor processing methods that include forming a first oxygen-containing material on a substrate. The first oxygen-containing material may be or include silicon oxide, yttrium oxide, or aluminum oxide. The method includes forming a barrier layer on the first oxygen-containing material. The method includes forming a second oxygen-containing material on the barrier layer. The second oxygen-containing material may be or include silicon oxide, yttrium oxide, or aluminum oxide.

[0007] In some embodiments, the first oxygen-containing material and the second oxygen-containing material may be or include the same material. The substrate may include a metal component of a semiconductor processing chamber. The barrier layer may be characterized by a thickness of less than or about 25 nm. The thickness of the barrier layer may be less than or about 20% of the combined thickness of the first oxygen-containing material, the barrier layer, and the second oxygen-containing material. The barrier layer may be or include hafnium oxide, lanthanum oxide, aluminum oxide, tungsten, tungsten nitride, or titanium nitride. The barrier layer may be deposited by atomic layer deposition. The method may include exposing the substrate to a halogen-containing species after forming the second oxygen-containing material. The barrier layer may reduce the number of corrosive components that interact with the substrate.

[0008] Some embodiments of the present technology may include semiconductor processing methods. The method may include i) forming an oxygen-containing material on a metal substrate. The oxygen-containing material may be or include silicon oxide, yttrium oxide, or aluminum oxide. The method may include ii) forming a barrier material. The barrier material may cover the oxygen-containing material. The method may include iii) repeating operations i and ii to form an alternating stack of oxygen-containing material and barrier material on the metal substrate.

[0009] In some embodiments, a temperature is maintained at less than or about 450° C. while forming the oxygen-containing material and the barrier material. The metal substrate may include stainless steel or aluminum semiconductor processing chamber components. The alternating stack may include more than three layers of barrier material. Each barrier material may be characterized by a thickness less than or about 10% of the total thickness of the alternating stack of oxygen-containing material and barrier material. The method may include iv) exposing the substrate to a halogen-containing species. The halogen-containing species may include fluorine. The oxygen-containing material may be or include yttrium oxide and the barrier material may be or include lanthanum oxide.

[0010] Some embodiments of the present technology include semiconductor structures. The structure may include a substrate. The structure may include an oxygen-containing material on the substrate. The oxygen-containing material may be or include silicon oxide, yttrium oxide, or aluminum oxide. The structure may include one or more barrier layers inserted into the oxygen-containing material. Each of the one or more barrier layers may be characterized by a thickness of less than or about 25 nm. The total thickness of the one or more barrier layers may be less than or about 50% of the combined thickness of the oxygen-containing material and the one or more barrier layers.

[0011] In some embodiments, the combined thickness of the oxygen-containing material and the one or more barrier layers may be between about 100 nm and about 500 nm. The substrate may include a metal substrate. Each of the one or more barrier layers may be conformally formed on the oxygen-containing material. The one or more barrier layers may be or include hafnium oxide, lanthanum oxide, aluminum oxide, tungsten, tungsten nitride, or titanium nitride.

[0012] The present technology provides many benefits over conventional corrosion resistant coatings for metal parts exposed to highly corrosive environments. Embodiments of the present technology form corrosion resistant coatings that can withstand highly corrosive halogen-containing atmospheres. In embodiments, the multilayer corrosion resistant coating includes one or more barrier layers inserted within a primary layer. A corrosion resistant primary layer such as silicon dioxide or yttrium oxide can resist corrosion from aggressive halogen-containing species in, for example, semiconductor manufacturing equipment. Additional barrier layers, such as metal oxides, metals, or metal nitrides, further increase the corrosion resistance of the corrosion resistant primary layer, thereby forming a highly corrosion resistant multilayer coating. The barrier layer can also reduce the outward migration of contaminant species from the substrate on which the multilayer coating is formed. These and other embodiments and their advantages and features are described in more detail in the following description and accompanying drawings in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] A further understanding of the nature and advantages of the disclosed technology may be realized by reference to the remaining portions of the specification and the drawings.

[0014] Figure 1 Selected operations in a method of forming a part are shown according to some embodiments of the present technology.

[0015] Figure 2 A diagrammatic cross-sectional view of a portion of a component coated with a multi-layer corrosion resistant coating in accordance with an embodiment of the present technology is shown.

[0016] Figure 3 A diagrammatic cross-sectional view of a portion of a component coated with a multi-layer corrosion resistant coating in accordance with additional embodiments of the present technology is shown.

[0017] Several drawings are included as diagrams. It will be understood that the drawings are for illustration purposes only and are not to be considered to be to scale unless expressly indicated as to scale. Furthermore, as diagrams, the drawings are provided to aid understanding and may not include all aspects or information compared to actual representations and may include exaggerated material for illustration purposes.

[0018] In the accompanying drawings, similar components and / or features may have the same reference numerals. Furthermore, various components of the same type may be distinguished by a letter following the reference numeral, which letter is used to distinguish similar components. If only the primary reference numeral is used in the specification, the description may apply to any of the similar components having the same primary reference numeral, regardless of the letter. DETAILED DESCRIPTION

[0019] Semiconductor processing includes operations to produce complex patterned materials on substrates. Operations include remote and in-situ formation and removal processes that utilize corrosive materials, including hot gases and ion plasmas containing halogen compounds, free radicals, and ions. For example, etching operations typically involve contacting substrates with halogen-containing liquids, gases, or plasma etchants that flow into a processing area of ​​a processing device. Although halogen-containing etchants are intended to etch wafers and other device substrates, they also react with the walls of the processing chamber and other equipment components to produce equipment corrosion. When equipment components are made of metals such as stainless steel or aluminum, halogen-containing materials react rapidly to cause equipment wear and become a source of contaminants. This contaminant can travel from the component to the substrate, contaminating the substrate and thereby affecting the final device performance. In addition, over time, this corrosion increases equipment repair and replacement costs and increases downtime for processing equipment.

[0020] Deposition processing may similarly use plasma enhanced processing or rapid thermal processing to form or deposit materials on substrates, which may also be deposited on chamber components. Once the substrate has been removed from the chamber, this will require a cleaning operation. The cleaning process may include utilizing one or more halogen-containing precursors or plasma effluents of these precursors to remove materials deposited on surfaces in the processing chamber. Although this cleaning will target the deposited materials, many exposed chamber component surfaces will be similarly attacked. For example, once the substrate has been removed from the processing chamber, the central area of ​​the substrate support without residual deposition material will be exposed. This cleaning process may begin to form a depression or other removal of the substrate support, which will reduce the flatness and integrity of the chuck. Many of these chamber components include multiple pieces joined together to create channels, flow paths, or sealing areas within the components. Individual pieces or combinations of equipment components within the chamber may be characterized by any number of internal features, including channels, pores, and various other morphologies.

[0021] Conventional technology has struggled to limit both corrosion and erosion of chamber components and has tended to replace components regularly due to damage caused by one or both of these mechanisms. Although some processes may include a seasoning process prior to semiconductor substrate processing, this can cause additional challenges. For example, the seasoning process may cover portions of the substrate support, but will not completely cover the backside or trunk, so components of the substrate support, such as the backplate or trunk, remain exposed to processing and cleaning materials. In addition, the seasoning process typically deposits a coating of one hundred nanometers or less. This can require replacing the seasoning for each substrate processed, which can increase queue time and also reduce the likelihood of uniform or complete coverage. Conventional technology has attempted to protect many of these components with coatings that are less reactive to corrosive materials and / or that can be more tolerant of plasma strikes.

[0022] Embodiments of the present technology solve these and other problems by coating chamber components with a multi-layer anti-corrosion coating that also prevents chamber components from contaminating structures being processed within the chamber. In an embodiment, the multi-layer coating includes a barrier layer formed between primary layers. In further embodiments, the multi-layer coating may include multiple barrier layers inserted within the primary layer. When the components coated with the multi-layer coating are subjected to processing, such as in an environment using halogen-containing species, the primary layer can reduce corrosion of the substrate. However, in the event that any corrosion of the substrate does occur, the barrier layer prevents contaminants from escaping the multi-layer coating. If contaminants are allowed to escape the multi-layer coating, the contaminants can interact with the structures or devices being processed. The multi-layer coating of the present technology reduces the corrosive species (such as halogen-containing species) that reach the components, and simultaneously reduces any contaminants from the components from reaching the interior of the chamber.

[0023] The remainder of the specification identifies specific materials, components, and semiconductor processing methods according to the present technology. It will be readily appreciated that the methods, materials, components, and systems described herein can be applied to a variety of other methods, materials, components, and systems for the manufacture of other types of devices used in semiconductor device manufacturing and components in corrosion protection coating manufacturing systems or equipment. Therefore, the present technology is not limited to the coating methods, materials, components, and systems described herein. This specification will discuss the non-limiting operation of example coating methods and general components that can be coated according to embodiments of the present technology.

[0024] Figure 1 Selected operations in method 100 for coating a semiconductor component substrate according to an embodiment of the present technology are shown. Many of the operations of method 100 may, for example, be performed in any number of chambers or systems, including oxidation chambers and atomic layer deposition chambers, and any combination of the systems discussed, or they may be configured to perform the operations discussed for method 100. Method 100 may include one or more operations prior to the first described operation, including producing or preparing one or more parts or portions that can be joined, and parts that have been joined. For example, upstream processing may include casting or treating metal parts, and preparing one or more surfaces for coating operations. Method 100 may further include optional operations that may or may not be particularly relevant to embodiments of the present technology. For example, some embodiments of the present coating method that provide a broader or alternative scope of the present method may include one or more operations that do not occur or occur at different times in other embodiments of the present technology.

[0025] Will also unite Figure 2 The method 100 is illustrated by a cross-sectional view of a portion of a component 200 shown in FIG. The component 200 includes an embodiment of the present multi-layer anti-corrosion coating positioned on a surface of a substrate 205 that forms at least a portion of the component. Figure 2In the illustrated embodiment, the multilayer coating is a multilayer coating including a primary layer 210 and a barrier layer 215. It should be appreciated that additional layers may be formed below the substrate 205 and above the primary layer 210. It should also be appreciated that the interface between the layers may or may not have a distinct boundary. For example, a portion of the interface may include a combination of materials from two adjacent layers (such as the primary layer 210 and the barrier layer 215). In an embodiment of the present technology, the coated component includes one or more substrate surfaces on which the multilayer coating is formed. The substrate surface includes an exposed surface of the substrate that forms a bonding layer of the multilayer coating. The substrate may include one or more metals that are incorporated into at least a portion of the component, such as a wall of the component. In an embodiment, the metal substrate may be or include any number of components or component sections. In additional embodiments, the metal substrate may be incorporated into a component of a semiconductor processing system for performing semiconductor manufacturing operations that use corrosive liquids, gases, and plasmas. In yet additional embodiments, the metal substrate may be incorporated into semiconductor manufacturing equipment components, such as base plates or edge rings, fluid delivery components such as showerheads or cover plates, structural components such as spacers or gaskets, and other single-piece or multi-piece components of semiconductor manufacturing equipment that can be coated according to the present method. The components may be substantially planar or may include complex geometries, which may include channels, pores, or other features throughout one or more surfaces of the components. The components may be made of any number of materials, which may be or include aluminum, carbon, chromium, copper, iron, magnesium, manganese, nickel, silicon, titanium, or zinc. The components may be or include alloys such as iron alloys, which may include any number of materials. In many embodiments, the metal substrate in the component includes stainless steel, such as 316 stainless steel. Although the discussion below may refer to components that may be made of stainless steel according to embodiments of the present technology, it will be understood that the present technology may be utilized with any iron alloy, and alloys of any number of other metals that may be used in semiconductor processing chambers or systems.

[0026] In an embodiment, the method 100 may include preparing the surface of the substrate 205 at optional operation 105. In further embodiments, this preparation may include removing an existing coating from the substrate surface, roughening the substrate surface, smoothing the substrate surface, exposing the substrate surface to an oxidizing environment, exposing the substrate surface to a passivating environment, and exposing the substrate surface to an etching environment, among other preparations. In some embodiments, since the substrate surface has already been prepared to form a multi-layer coating, the substrate surface preparation at optional operation 105 may be omitted.

[0027] In additional embodiments, substrate surface preparation at optional operation 105 may include removing oxides, organics, oils, dirt, particles, debris, and / or other contaminants from the surface of substrate 205. In further embodiments, the preparation may include sandblasting or texturing the surface, exposing the surface to a vacuum, solvent cleaning the surface, acid cleaning the surface, wet cleaning the surface, plasma cleaning the surface, and ultrasonicating the surface, among other preparations. The prepared surface of substrate 205 may be characterized by faster formation and stronger bonding of multi-layer coatings on the surface compared to an unprepared substrate surface.

[0028] In further embodiments, preparation of the substrate surface may include sandblasting or exposing the surface to one or more types of abrasive particles, such as beads, sand, and carbonates, solid carbon dioxide (CO 2 ), among other particle types. In embodiments, this particle exposure removes oxides and other contaminants from the substrate surface and may also provide texturing of the surface of the substrate 205. In further embodiments, preparation of the substrate surface may include placing the component 200 into a chamber within a pulsed push-pull gas circulation system and exposing the substrate surface of the component to at least one cycle of a purge gas such as nitrogen, argon, helium, and mixtures of the foregoing. In further embodiments, the component 200 may be exposed to at least one vacuum purge to remove particles and other debris from the substrate surface. In yet further embodiments, the component 200 may be placed into a plasma chamber and the substrate surface may be exposed to one or more types of plasmas, such as hydrogen-containing plasmas, oxygen- or ozone-containing plasmas, and nitrogen-containing plasmas, among other types of plasmas. In yet further embodiments, the plasma may be generated in situ, or may be remotely generated outside of the chamber holding the component 200 and delivered to the chamber.

[0029] In more embodiments, the preparation of the substrate surface may include removing one or more organic compounds and oxide compounds from the surface of the substrate 205. In additional embodiments, organic and oxide compounds may be removed from the surface by a reducing plasma such as a hydrogen plasma. In more embodiments, the reduced organic and oxide compounds may be degassed from the surface and exposed to ozone. In still more embodiments, the preparation of the substrate surface may include wet cleaning to remove organic compounds from the surface. In embodiments, wet cleaning may include soaking the substrate surface in an alkaline degreasing solution, rinsing, exposing the surface to an acidic cleaning (e.g., sulfuric acid, phosphoric acid, or hydrochloric acid), rinsing again, and exposing the surface to a deionized water ultrasonic oscillation bath. In yet additional embodiments, the preparation of the substrate surface may include wet cleaning to remove oxide compounds from the surface. In embodiments, wet cleaning may include exposing the substrate surface to a dilute acidic solution (e.g., acetic acid or hydrochloric acid), rinsing, and exposing the surface to deionized water in an ultrasonic oscillation bath. In further embodiments, the preparation of the substrate surface may include a preparation operation to remove particles from the substrate surface. In one embodiment, these particle removal preparations may include exposing the substrate surface to ultrasonic vibrations (e.g., megasonic vibrations) and / or supercritical carbon dioxide washing, followed by exposure to a purge gas (e.g., N 2 , Ar, He, or any combination of the foregoing) and a cycle of vacuum purge to remove particles from the surface and dry the surface. In yet further embodiments, preparation of the substrate surface may include exposing the surface to a heating and drying operation. In an embodiment, the heating operation may include exposing the substrate surface to a temperature exceeding room temperature. In additional embodiments, the elevated temperature may be characterized by a temperature greater than or about 50°C, greater than or about 75°C, greater than or about 100°C, greater than or about 125°C, greater than or about 150°C, greater than or about 175°C, greater than or about 200°C, or greater. In more embodiments, the heating operation may include exposing the substrate surface to a heat lamp or placing the component in a furnace.

[0030] The method 100 may further include forming a main layer 210, such as a first portion or a first oxygen-containing material of the main layer 210, on the substrate 205 at operation 110. In an embodiment, the oxygen-containing material of the main layer 210 may include silicon oxide, such as silicon dioxide. In further embodiments, the silicon oxide (e.g., SiO 2) may be greater than or about 50 wt.%, greater than or about 60 wt.%, greater than or about 70 wt.%, greater than or about 80 wt.%, greater than or about 90 wt.%, greater than or about 95 wt.%, or more of the total weight of the primary layer 210. In still further embodiments, the primary layer 210 may be deposited by a vapor deposition process, such as atomic layer deposition (ALD), plasma enhanced atomic layer deposition (PE-ALD), thermal chemical vapor deposition (CVD), and plasma enhanced chemical vapor deposition (PE-CVD), among other vapor deposition processes. In further embodiments, the deposition process may include an ALD process that provides a semiconductor reactant or a metal-containing reactant and an oxidizing reactant to a deposition process region, where these reactants form a silicon oxide-containing layer on at least a portion of the substrate 205. The semiconductor reactant or the metal-containing reactant and the oxidizing reactant deposit the primary layer 210 on the substrate 205. In additional embodiments, the semiconductor reactant or metal-containing reactant may include a silicon-containing reactant such as silane, silicon chloride, silicon cyanate, oxysilane, or aminosilane, among other silicon-containing reactants. In yet additional embodiments, the silane may include one or more of silane, disilane, trisilane, tetrasilane, pentasilane, and hexasilane, among other silanes. In yet further embodiments, silicon chloride may include one or more of monochlorosilane, dichlorosilane, trichlorosilane, tetrachlorosilane, and hexachlorosilane, among other silicon chlorides. In more embodiments, silicon cyanate may include tetraisocyanatosilane, among other silicon cyanates. In yet more embodiments, oxysilane may include tetraethoxysilane, among other oxysilanes. In additional embodiments, aminosilane may include tris(dimethyloamino)silane, bis(ethyl-methylamino)silane, among other aminosilanes. In additional embodiments, the oxidation reactant may include water (e.g., steam), oxygen (O 2 ), atomic oxygen (O), ozone (O 3 ), nitrous oxide, one or more peroxides, one or more alcohols, plasmas of the foregoing, or any combination of the foregoing. In further embodiments, one or both of the silicon-containing reactant and the oxidizing reactant may include one or more carrier gases, such as nitrogen (N 2 ), argon, helium, neon, and hydrogen (H 2 ), other carrier gases.

[0031] In further embodiments, atomic layer deposition of the main layer 210 may include one or more cycles of exposing the substrate 205 to a semiconductor-containing or metal-containing reactant, performing a purge pump operation of the deposition process area to remove residual metal-containing reactant, exposing the component to an oxidizing reactant, and performing another purge pump operation to remove residual oxidizing reactant from the deposition process area. In still more embodiments, the ALD operation may include greater than or about 1 cycle, greater than or about 2 cycles, greater than or about 3 cycles, greater than or about 4 cycles, greater than or about 5 cycles, greater than or about 8 cycles, greater than or about 10 cycles, greater than or about 15 cycles, greater than or about 20 cycles, greater than or about 30 cycles, greater than or about 50 cycles, greater than or about 80 cycles, greater than or about 100 cycles, greater than or about 150 cycles, greater than or about 200 cycles, greater than or about 250 cycles, greater than or about 300 cycles, greater than or about 350 cycles, greater than or about 400 cycles, greater than or about 450 cycles, greater than or about 500 cycles, or more. In yet more embodiments, each cycle may deposit a portion of the main layer 210 characterized by a thickness of less than or about 25 nm, less than or about 20 nm, less than or about 17.5 nm, less than or about 15 nm, less than or about 12.5 nm, less than or about 10 nm, less than or about 7.5 nm, less than or about 5 nm, or less.

[0032] In additional embodiments, the oxygen-containing material of the primary layer 210 may include yttrium oxide, such as yttrium trioxide. In further embodiments, the yttrium oxide (e.g., Y 2 O 3) may be greater than or about 50 wt.%, greater than or about 60 wt.%, greater than or about 70 wt.%, greater than or about 80 wt.%, greater than or about 90 wt.%, greater than or about 95 wt.%, or more of the total weight of the primary layer 210. Similar to the silicon oxide materials discussed previously, the yttrium oxide may be deposited by a vapor deposition process, such as ALD, PE-ALD, CVD, and PE-CVD, among other vapor deposition processes. In further embodiments, the deposition process may include an ALD process that provides a semiconductor-containing or metal-containing reactant and an oxidizing reactant to a deposition process region where they form a yttrium oxide-containing layer on at least a portion of the substrate 205. The semiconductor-containing or metal-containing reactant and the oxidizing reactant deposit the primary layer 210 on the substrate 205. In additional embodiments, the semiconductor-containing or metal-containing reactant may include a yttrium-containing reactant, such as tris(N,N-bis(trimethylsilyl)amide)yttrium(III), yttrium(III)butoxide, yttrium(III)chloride, tris(methylcyclopentadienyl)yttrium, tris(butylcyclopentadienyl)yttrium, tris(cyclopentadienyl)yttrium, and yttrium-containing reactants other than these.

[0033] In yet more embodiments, the oxygen-containing material of the main layer 210 may include aluminum oxide. In further embodiments, the aluminum oxide (e.g., Al 2 O 3) may be greater than or about 50 wt.%, greater than or about 60 wt.%, greater than or about 70 wt.%, greater than or about 80 wt.%, greater than or about 90 wt.%, greater than or about 95 wt.%, or more of the total weight of the barrier layer 215. In still further embodiments, the primary layer 210 containing aluminum oxide may be deposited by a vapor deposition process, such as ALD, PE-ALD, CVD, and PE-CVD, among other vapor deposition processes. In further embodiments, the deposition process may include an ALD process that provides a semiconductor-containing or metal-containing reactant and an oxidizing reactant to a deposition process zone where they form an aluminum oxide-containing layer on at least a portion of the substrate 205. The semiconductor-containing or metal-containing reactant and the oxidizing reactant deposit the primary layer 210 on the substrate 205. In additional embodiments, the semiconductor-containing or metal-containing reactant may include an aluminum-containing reactant, such as one or more aluminum alkyl compounds, one or more aluminum alkoxy compounds, and one or more aluminum acetylacetonate compounds, among other aluminum-containing reactants. In yet more embodiments, the aluminum-containing reactant may include trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, trimethoxyaluminum, triethoxyaluminum, tripropoxyaluminum, tributoxyaluminum, acetylacetonate aluminum (Al(acac) 3 , also known as aluminum tris(2,4-pentanedione)), aluminum hexafluoroacetylacetonate (Al(hfac) 3 ), and trisdipivaloylmethanatoaluminum (DPM 3 Al; (C 11 H 19 O 2 ) 3 Al)), other aluminum-containing reactants.

[0034] The method 100 may further include forming a barrier layer 215 at operation 115. The barrier layer 215 may be conformally formed on the main layer 210. In an embodiment, the barrier layer 215 may include hafnium oxide. In further embodiments, the hafnium oxide (e.g., HfO) in the barrier layer 215 may be formed on the main layer 210 in a conformal manner. 2) may be greater than or about 50 wt.%, greater than or about 60 wt.%, greater than or about 70 wt.%, greater than or about 80 wt.%, greater than or about 90 wt.%, greater than or about 95 wt.%, or more of the total weight of the barrier layer 215. In still further embodiments, the barrier layer 215 containing hafnium oxide may be deposited by a vapor deposition process, such as ALD, PE-ALD, CVD, and PE-CVD, among other vapor deposition processes. In further embodiments, the deposition process may include an ALD process that provides a hafnium-containing reactant and an oxidizing reactant to a deposition process region that has at least a portion of the primary layer 210 exposed to be formed on the component 200. In additional embodiments, the hafnium-containing reactant may include a cyclopentadienyl hafnium compound, an amine hafnium compound, an alkyl hafnium compound, and an alkoxy hafnium compound, among other hafnium-containing reactants. In further embodiments, the hafnium-containing reactant may include bis(methylcyclopentadiene)dimethylhafnium ((MeCp) 2 HkDJ 2 )), bis(methylcyclopentadiene)methylmethoxyhafnium((MeCp) 2 Hf(OMe)(Me))), bis(cyclopentadiene)dimethylhafnium((Cp) 2 HkDJ 2 )), tetra(tert-butoxy)hafnium, hafnium isopropoxide((iPrO) 4 Hf)), tetrakis(dimethylamino)hafnium (TDMAH)), tetrakis(diethylamino)hafnium (TDEAH)), and tetrakis(ethylmethylamino)hafnium (TEMAH), and other hafnium-containing reactants.

[0035] In further embodiments, the barrier layer 215 may include lanthanum oxide. In further embodiments, the lanthanum oxide (eg, HfO 2) may be greater than or about 50 wt.%, greater than or about 60 wt.%, greater than or about 70 wt.%, greater than or about 80 wt.%, greater than or about 90 wt.%, greater than or about 95 wt.%, or more of the total weight of the barrier layer 215. In still further embodiments, the barrier layer 215 comprising a lanthanum oxide may be deposited by a vapor deposition process, such as ALD, PE-ALD, CVD, and PE-CVD, among other vapor deposition processes. In further embodiments, the deposition process may include an ALD process that provides a lanthanum-containing reactant and an oxidizing reactant to a deposition process zone that has at least a portion of the primary layer 210 exposed to be formed on the component 200. In additional embodiments, the lanthanum-containing reactant may include lanthanum cyclopentadienyl compounds, lanthanum amide compounds, lanthanum alkyl compounds, and lanthanum alkoxide compounds, among other lanthanum-containing reactants. In further embodiments, the lanthanum-containing reactant may include lanthanum (III) chloride, tris(i-propylcyclopentadienyl) lanthanum, tris(cyclopentadienyl) lanthanum, lanthanum (III) i-propoxide, lanthanum (III) acetylacetonate hydrate, tris(N,N-di-i-propylpentylamidinato) lanthanum (III), tris(N,N-bis(trimethylsilyl)amide) lanthanum (III), tris(N,N'-di-i-propylformamidinato) lanthanum (III), and tris(N,N'-di-i-propylformamidinato) lanthanum (III). II)), tris(6,6,7,7,8,8,8-heptafluoro-2,2-dimethyl-3,5-octanedionate)lanthanum(III)), tris(2,2,6,6-tetramethyl-3,5-heptanedionato)lanthanum(III), and other lanthanum-containing reactants.

[0036] In yet additional embodiments, barrier layer 215 may include oxides of one or more metals, such as aluminum, chromium, magnesium, nickel, titanium, and zirconium, among other metals.

[0037] In further embodiments, the barrier layer 215 may include tungsten. The tungsten in the barrier layer 215 may be greater than or about 50 wt.%, greater than or about 60 wt.%, greater than or about 70 wt.%, greater than or about 80 wt.%, greater than or about 90 wt.%, greater than or about 95 wt.%, or more of the total weight of the barrier layer 215. In still further embodiments, the tungsten-containing barrier layer 215 may be deposited by a vapor deposition process, such as ALD, PE-ALD, CVD, and PE-CVD, among other vapor deposition processes. In further embodiments, the deposition process may include an ALD process that provides a tungsten-containing reactant and a hydrogen-containing co-reactant to a deposition process region that has at least a portion of the main layer 210 exposed to be formed on the component 200. The hydrogen-containing co-reactant may only serve as a sacrificial role to strip material from the tungsten without being incorporated into the film. In additional embodiments, the tungsten-containing reactant may include one or more of tungsten disulfide, tungsten hexafluoride, tungsten pentafluoride, among other tungsten-containing reactants. In additional embodiments, the hydrogen-containing co-reactant may include one or more of silane, disilane, trisilane, or any other hydrogen-containing reactant.

[0038] In yet additional embodiments, barrier layer 215 may include one or more additional metals, such as aluminum, chromium, magnesium, nickel, titanium, and zirconium, among other metals.

[0039] In yet more embodiments, the barrier layer 215 may include tungsten nitride. The tungsten nitride (e.g., W) in the barrier layer 215 2 N, WN, WN 2 ) may be greater than or about 50 wt.%, greater than or about 60 wt.%, greater than or about 70 wt.%, greater than or about 80 wt.%, greater than or about 90 wt.%, greater than or about 95 wt.%, or more of the total weight of the barrier layer 215. In still further embodiments, the barrier layer 215 comprising tungsten nitride may be deposited by a vapor deposition process, such as ALD, PE-ALD, CVD, and PE-CVD, among other vapor deposition processes. In further embodiments, the deposition process may include an ALD process that provides a tungsten-containing reactant and a nitrogen-containing reactant to a deposition process region that has at least a portion of the primary layer 210 exposed to be formed on the component 200. In additional embodiments, the tungsten-containing reactant may include one or more of tungsten disulfide, tungsten hexafluoride, tungsten pentafluoride, among other tungsten-containing reactants. In additional embodiments, the nitrogen-containing reactant may include one or more of diatomic nitrogen, a combination of diatomic nitrogen and diatomic hydrogen, ammonia, a plasma of the foregoing, or any other nitrogen-containing reactant.

[0040] In yet more embodiments, the barrier layer 215 may include titanium nitride. The titanium nitride (e.g., TiN) in the barrier layer 215 may be greater than or about 50 wt.%, greater than or about 60 wt.%, greater than or about 70 wt.%, greater than or about 80 wt.%, greater than or about 90 wt.%, greater than or about 95 wt.%, or more of the total weight of the barrier layer 215. In yet further embodiments, the barrier layer 215 comprising titanium nitride may be deposited by a vapor deposition process, such as ALD, PE-ALD, CVD, and PE-CVD, among other vapor deposition processes. In further embodiments, the deposition process may include an ALD process that provides a titanium-containing reactant and a nitrogen-containing reactant to a deposition process region that has at least a portion of the primary layer 210 exposed to be formed on the component 200. In additional embodiments, the titanium-containing reactant may include titanium tetrachloride (TiCl 4 In some embodiments, the nitrogen-containing reaction may include one or more of diatomic nitrogen, a combination of diatomic nitrogen and diatomic hydrogen, ammonia, a plasma of the foregoing, or any other nitrogen-containing reactant.

[0041] In yet additional embodiments, barrier layer 215 may include nitrides of one or more additional metals, such as aluminum, chromium, magnesium, nickel, and zirconium, among other metals.

[0042] The temperature when forming the main layer 210 and / or the barrier layer 215 can be maintained at less than or about 450° C. Since the layers can be deposited by ALD, higher temperatures can cause the precursors used to form the layers to decompose before being deposited on the surface of the substrate 205 and / or the main layer 210, which can affect the deposition. Therefore, the temperature can be maintained at less than or about 400° C., less than or about 350° C., less than or about 300° C., less than or about 250° C., less than or about 200° C., less than or about 150° C., less than or about 100° C., or less.

[0043] The method 100 may further include repeatedly forming portions of the primary layer 210 and the barrier layer 215 at optional operation 120. Figure 2 200, the component 200 includes three barrier layers 215 disposed between four portions of the primary layer 210. Although the primary layer 210 is depicted as contacting the substrate 205, it is contemplated that the barrier layer 215 may alternatively contact the substrate 205. Similarly, although the primary layer 210 is depicted as the uppermost layer on the component 200, it is contemplated that the barrier layer 215 may alternatively be the uppermost layer. In embodiments, the component may include any number of alternating layers of the primary layer 210 and the barrier layer 215. For example, the component 200 may include greater than three layers of barrier material, greater than four layers of barrier material, greater than five layers of barrier material, greater than ten layers of barrier material, greater than fifteen layers of barrier material, greater than twenty layers of barrier material, greater than twenty-five layers of barrier material, greater than thirty layers of barrier material, greater than thirty-five layers of barrier material, or more.

[0044] The method 100 may further include forming an additional primary layer 210, such as a second portion of the primary layer 210 or a second oxygen-containing material, on the barrier layer 215 at operation 125. In an embodiment, the second portion of the primary layer 210 formed at operation 125 may be the same material formed at operation 110. For example, when silicon oxide is formed at operation 110, additional silicon oxide may be formed over the barrier layer 215 at operation 125. However, it is contemplated that the primary layer 210 may include different materials on opposite sides of the barrier layer 215.

[0045] In embodiments, the corrosion resistance of the coated component 200 can be increased by increasing the thickness of the primary layer 210 and / or the barrier layer 215. The more material the corrosive species must penetrate or remove to reach the surface of the substrate 205, the longer the coated component can resist the corrosive effects of the corrosive species. In further embodiments, the multilayer coating including the primary layer 210 and the barrier layer 215 can be characterized by a thickness of greater than or about 50 nm, greater than or about 75 nm, greater than or about 100 nm, greater than or about 125 nm, greater than or about 150 nm, greater than or about 175 nm, greater than or about 200 nm, greater than or about 225 nm, greater than or about 250 nm, greater than or about 275 nm, greater than or about 300 nm, greater than or about 350 nm, greater than or about 400 nm, greater than or about 450 nm, greater than or about 500 nm, or greater. Since many embodiments include ALD deposition, which may require significant processing time, the multilayer coating may be characterized by a thickness of less than or about 750 nm, less than or about 700 nm, less than or about 650 nm, less than or about 600 nm, less than or about 550 nm, less than or about 500 nm, less than or about 450 nm, less than or about 400 nm, less than or about 350 nm, less than or about 300 nm, less than or about 250 nm, less than or about 200 nm, less than or about 150 nm, less than or about 100 nm, or less. In embodiments, the combined thickness of the primary layer 210, such as an oxygen-containing material, and the one or more barrier layers 215 may be between about 100 nm and about 500 nm.

[0046] In additional embodiments, the barrier layer 215 may be characterized by a thickness of less than or about 25 nm, less than or about 20 nm, less than or about 17.5 nm, less than or about 15 nm, less than or about 12.5 nm, less than or about 10 nm, less than or about 7.5 nm, less than or about 5 nm, or less. In further embodiments, the thickness of the barrier layer 215 may be related to the thickness of the multilayer coating, which may include any portion of the primary layer 210 (e.g., oxygen-containing material) and the barrier layer 215. For example, the thickness of the barrier layer 215 may be less than or about 20% of the combined thickness of the multilayer coating, such as less than or about 17.5%, less than or about 15%, less than or about 12.5%, less than or about 10%, less than or about 7.5%, less than or about 5%, or less. In embodiments having multiple barrier layers 215, the total thickness of one or more barrier layers 215 may be less than or about 50% of the combined thickness of the multilayer coating, such as less than or about 45%, less than or about 40%, less than or about 35%, less than or about 30%, less than or about 25%, less than or about 20%, less than or about 15%, less than or about 10%, less than or about 5%, or less.

[0047] The method 100 may include exposing the component 200 having the multi-layer coating to one or more corrosive substances at optional operation 130. The one or more corrosive substances may include halogen-containing species, such as fluorine, chlorine, and bromine. In an embodiment, the halogen-containing species may be included in a halogen-containing compound, free radical, or ion, incorporated into a halogen-containing liquid, solution, precursor, gas, or plasma, or in a halogen-containing medium. For example, the chlorine-containing corrosive substance may include hydrogen chloride or hydrochloric acid (HCl), molecular chlorine (Cl 2 ), chlorine radicals (Cl), and oxygen-containing and chlorine compounds, nitrogen-containing and chlorine compounds, and carbon-containing and chlorine compounds, and other chlorine-containing substances. For example, the fluorine-containing corrosive substances may include nitrogen trifluoride (NF 3 ), sulfur hexafluoride (SF 6 ), carbon tetrafluoride (CF 4 ), hexafluoroethane, other carbon- and fluorine-containing compounds, and one or more of other fluorine-containing substances.

[0048] The primary layer 210 and / or barrier layer 215 can be characterized by a higher corrosion resistance to one or more corrosive species relative to the substrate 205 of the component 200. In embodiments, the halogen etch rate ratio of the substrate surface relative to the primary layer 210 and / or barrier layer 215 can be characterized by greater than or about 10:1, greater than or about 50:1, greater than or about 100:1, greater than or about 200:1, greater than or about 300:1, greater than or about 400:1, greater than or about 500:1, greater than or about 600:1, greater than or about 700:1, greater than or about 800:1, greater than or about 900:1, greater than or about 1000:1, or greater. In additional embodiments, the primary layer 210 and / or barrier layer 215 can reduce the corrosion rate of the coated component from chlorine-containing corrosive species compared to the corrosion rate of the substrate 205 of the uncoated component. In yet additional embodiments, the barrier layer 215 may reduce the corrosion rate of the coated components to less than or about 90%, less than or about 80%, less than or about 70%, less than or about 60%, less than or about 50%, less than or about 40%, less than or about 30%, less than or about 20%, less than or about 10%, less than or about 5%, less than or about 1%, or less of the corrosion rate of the uncoated components.

[0049] In an embodiment, the barrier layer 215 can reduce the ability of contaminants from the substrate 205 to travel through the multi-layer coatings of the component 200. If the halogen-containing species do reach the substrate 205 and cause any corrosion, the barrier layer 215 can reduce or prevent any formed contaminants from traveling through the multi-layer coatings. If contaminants are able to travel through the multi-layer coatings, these contaminants can interact with structures such as wafers that are processed in proximity to the component 200. Such contamination of nearby structures can result in reduced performance of the processed structures and / or the final device.

[0050] Figure 3 A cross-sectional view of a portion of a component 300 coated with a multi-layer corrosion resistant coating according to an additional embodiment of the present invention is shown. The substrate 305 of the component 300 includes stages to illustrate the conformality of the primary layer 310 and the barrier layer 315 to the shape of the substrate of the component, among other aspects, of the stages, grooves, pores, channels, fluid paths, tubes, and openings. In embodiments, the present technology includes forming a conformal coating that can extend over any of the various features and aspects of the component. In embodiments, the conformality of the coating can be characterized by low variation in the thickness of the multi-layer coating on orthogonal surfaces of the stages in the substrate 305. In embodiments, the variation in the thickness of the multi-layer coating between orthogonal surfaces can be characterized by less than or about 10%, less than or about 7.5%, less than or about 5%, less than or about 2.5%, less than or about 1%, or less.

[0051] In additional embodiments, component 300 may include one or more pores (not shown) characterized by an aspect ratio (i.e., height to width ratio) of greater than or about 1:1, greater than or about 2:1, greater than or about 3:1, greater than or about 4:1, greater than or about 5:1, greater than or about 6:1, greater than or about 7:1, greater than or about 8:1, greater than or about 10:1, or greater. In yet additional embodiments, the multilayer coating may be characterized by a high degree of uniformity on the inner walls of the pores compared to other portions of the coating. In embodiments, the uniformity of the multilayer coating between the inner walls of the pores and other portions of the coating may be characterized by having thicknesses within 90% of each other and may be characterized by thicknesses within 92% of each other, thicknesses within 94% of each other, thicknesses within 96% of each other, thicknesses within 98% of each other, thicknesses within 99% of each other, or substantially equal to each other within the error range of any measurement device or technique used.

[0052] The present technology includes components, such as metal-containing chamber components, coated with a multilayer coating that provides increased corrosion resistance to such components. In embodiments, the multilayer coating includes one or more barrier layers that reduce the likelihood of contamination of structures or devices being processed in the chamber. The primary layer of the multilayer coating reduces the corrosive effects of corrosive species, such as halogen-containing species, on the coated components. The barrier layer reduces the likelihood of contaminants from the components reaching the chamber in the event of corrosion. If the barrier layer does not exist to prevent contaminants from the coated components from traveling away from the multilayer coating, these contaminants would negatively affect operations within the chamber by contaminating the structures or devices being processed. In embodiments, components coated with the present multilayer coating have an extended operating life compared to uncoated components and also prevent contaminants from the components from traveling through the multilayer coating.

[0053] In the foregoing description, for the purpose of explanation, many details have been described to provide an understanding of various embodiments of the present technology. However, it is apparent to one skilled in the art that a specific embodiment can be implemented without some of these details or with additional details.

[0054] Several embodiments have been disclosed, and those skilled in the art will recognize that various modifications, alternative architectures, and equivalents may be used without departing from the spirit of the embodiments. In addition, several well-known processes and components are not described to avoid unnecessary confusion of the present technology. Therefore, the above description should not be taken as limiting the scope of the present technology.

[0055] When a numerical range is provided, unless the context clearly indicates otherwise, it is understood that each intervening value between the upper and lower limits of the range to the smallest fraction of a unit of the lower limit is also explicitly disclosed. Any narrower range between any stated value or unstated intervening value in the stated range and any other stated or intervening value in the stated range is covered. The upper and lower limits of those smaller ranges may be independently included or excluded in this range, and subject to any explicitly excluded limits in the stated range, ranges in which any limit is included, none of the limits are included, or both of the limits are included in the smaller range are also covered in the present technology. When a stated range includes one or both of the limits, ranges excluding either or both of these included limits are also included.

[0056] As used herein and in the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to "a layer" includes a plurality of such layers and reference to "the precursor" includes reference to one or more precursors and equivalents thereof known to those skilled in the art, and so forth.

[0057] Furthermore, the words “comprise(s)”, “comprising”, “contain(s)”, “containing”, “include(s)”, and “including” when used in this specification and in the following claims are intended to indicate the presence of stated features, integers, components, or operations, but they do not exclude the presence or addition of one or more other features, integers, components, operations, actions, or groups.

Claims

1. A semiconductor processing method comprising the following steps: forming a first oxygen-containing material on a substrate, wherein the first oxygen-containing material comprises silicon oxide, yttrium oxide, or aluminum oxide; forming a barrier layer on the first oxygen-containing material; and A second oxygen-containing material is formed on the barrier layer, wherein the second oxygen-containing material comprises silicon oxide, yttrium oxide, or aluminum oxide. 2 . The semiconductor processing method of claim 1 , wherein the first oxygen-containing material and the second oxygen-containing material comprise the same material.

3. The semiconductor processing method of claim 1, wherein the substrate comprises a metal component of a semiconductor processing chamber.

4. The semiconductor processing method of claim 1 wherein the barrier layer is characterized by a thickness of less than or about 25 nm.

5. The semiconductor processing method of claim 1, wherein the thickness of the barrier layer is less than or about 20% of the combined thickness of the first oxygen-containing material, the barrier layer, and the second oxygen-containing material.

6. The semiconductor processing method of claim 1, wherein the barrier layer comprises hafnium oxide, lanthanum oxide, aluminum oxide, tungsten, tungsten nitride, or titanium nitride.

7. The semiconductor processing method of claim 1, wherein the barrier layer is deposited by atomic layer deposition.

8. The semiconductor processing method according to claim 1, further comprising the steps of: After forming the second oxygen-containing material, the substrate is exposed to a halogen-containing species, wherein the barrier layer reduces the amount of corrosive species that interact with the substrate.

9. A semiconductor processing method comprising the following steps: i) forming an oxygen-containing material on a metal substrate, wherein the oxygen-containing material comprises silicon oxide, yttrium oxide, or aluminum oxide; ii) forming a barrier material, wherein the barrier material covers the oxygen-containing material; and iii) repeating operations i and ii to form an alternating stack of oxygen-containing materials and barrier materials on the metal substrate.

10. The semiconductor processing method of claim 9, wherein a temperature is maintained at less than or about 450°C while forming the oxygen-containing material and the barrier material.

11. The semiconductor processing method of claim 9, wherein the metal substrate comprises a stainless steel or aluminum semiconductor processing chamber component.

12. The semiconductor processing method of claim 9 wherein the alternating stack comprises more than three layers of barrier material.

13. The semiconductor processing method of claim 9 wherein each barrier material is characterized by a thickness that is less than or about 10% of the total thickness of the alternating stack of oxygen-containing material and barrier material.

14. The semiconductor processing method of claim 9, further comprising the steps of: iv) exposing the substrate to a halogen-containing species.

15. The semiconductor processing method according to claim 14, in: The halogen-containing species comprises fluorine; The oxygen-containing material comprises yttrium oxide; and The barrier material includes lanthanum oxide.

16. A semiconductor structure comprising: substrate; an oxygen-containing material on the substrate, wherein the oxygen-containing material comprises silicon oxide, yttrium oxide, or aluminum oxide; and One or more barrier layers are inserted within the oxygen-containing material, wherein each of the one or more barrier layers is characterized by a thickness of less than or about 25 nm, and wherein the total thickness of the one or more barrier layers is less than or about 50% of the combined thickness of the oxygen-containing material and the one or more barrier layers.

17. The semiconductor structure of claim 16, wherein the combined thickness of the oxygen-containing material and the one or more barrier layers is between about 100 nm and about 500 nm.

18. The semiconductor structure of claim 16, wherein the substrate comprises a metal substrate.

19. The semiconductor structure of claim 16, wherein each of the one or more barrier layers is conformally formed on the oxygen-containing material.

20. The semiconductor structure of claim 16, wherein the one or more barrier layers comprise hafnium oxide, lanthanum oxide, aluminum oxide, tungsten, tungsten nitride, or titanium nitride.