Film for back panel, polyester film, and image display device and device on which film for back panel or polyester film is mounted
By using biaxially oriented polyester film as the back panel, the problems of color unevenness and insufficient heat resistance caused by plastic film are solved, and high-quality shooting quality and heat resistance are improved.
Patent Information
- Application Number
- CN202380035759.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-27
- Filing Date
- 2023-06-21
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, when using plastic film as the back panel, color unevenness is likely to occur, resulting in a decrease in image quality, and when configuring photoelectric conversion elements such as cameras, information quality is degraded, and heat resistance and bending resistance are insufficient.
Biaxially oriented polyester film is used as the back panel, and the phase difference value of the film is controlled to be 0 nm or more and 1000 nm or less, and contains 6 mol% or more isophthalic acid component, with a crystallinity of less than 30% or more and a rigidity of more than 20% or more. Amorphous amount and through specific heat treatment and stacked structure design, the bending rigidity and heat resistance of the film are improved.
Effectively suppress the generation of rainbow spots, improve shooting quality, optimize the information accuracy of photoelectric conversion elements, and improve the film's heat resistance and bending performance.
Smart Images

Figure CN119072644A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a back panel film for light emission for image display, a polyester film, an image display device, and a device having the image display device. Background Art
[0002] With the development of display terminals, image display devices are required to be small, thin, and lightweight.
[0003] Field luminescent display devices represented by organic light-emitting display devices are self-luminous display devices. Unlike liquid crystal display devices, they do not require an additional light source and are easy to achieve thinness and lightness. They are also excellent in terms of hue, response speed, field of view, and contrast ratio, and have been applied to display devices.
[0004] On the other hand, as display devices are miniaturized, they are expected to have large screens (large display areas), and the area other than the display area in the display device is also required to be reduced, and full-screen display in display terminals has attracted attention.
[0005] On the other hand, in smart phones and tablet terminals, cameras are often installed based on the need to take photos and save them in records or share them with friends. In such terminals, cameras are not only installed on the back side, but sometimes also on the image display side.
[0006] When a camera is arranged on the image display surface side, most of them are arranged in the form of a slit or an opening. That is, a hole or a slit is provided on the image display surface side for allowing light from the outside to enter the camera lens. When shooting, light from the outside passes through the slit or opening and enters the camera arranged below the image display surface. The area where such a slit or opening exists is a non-display area, and therefore, the development of an image display device without a slit or an opening is in progress (for example, Patent Document 1).
[0007] In addition, by reducing the frame area equivalent to the non-display area as the outer part of the display area and developing a foldable display device that can open and close multiple image display devices in a foldable form, the realization of large-screen display and the miniaturization and lightness of the terminal are studied. In their development, a flexible image display device is proposed with a thin film that can maintain display performance even when bent, but such an image display device is too thin, so there is a situation where it cannot be restored or the fold is fixed when bent. Therefore, in order to support it and maintain the curvature during bending within an appropriate range, as such a backplane configured at the bottom of the flexible substrate, a metal backplane such as stainless steel, a plastic backplane such as polymethyl methacrylate, polycarbonate, polyvinyl alcohol, and polyethylene terephthalate (for example, Patent Document 2) are known. In addition, it is known that for plastic films, color unevenness and rainbow spots sometimes occur due to the combination with specific components (polarizers, etc.), and various countermeasures have been made (for example, Patent Documents 3 to 5).
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application No. 2021-511649
[0011] Patent Document 2: Japanese Patent Application Publication No. 2021-107918
[0012] Patent Document 3: Japanese Patent Application Publication No. 2022-133016
[0013] Patent Document 4: Japanese Patent No. 6862654
[0014] Patent Document 5: Japanese Patent No. 6950731 Summary of the invention
[0015] Problems to be solved by the invention
[0016] However, it was found that when a specific plastic film is used as the back panel film, the following problem occurs: rainbow-shaped color unevenness occurs in the image obtained by the camera provided on the image display surface side without slits or openings. The generation of such color unevenness leads to a reduction in image quality. In addition, when other photoelectric conversion elements such as fingerprint authentication sensors, light sensors, and distance sensors are used instead of cameras, the quality of the obtained information is reduced. As an improvement to such color unevenness, as in the technology of Patent Document 3, a polarization elimination member is inserted between the camera and the plastic film to eliminate it, but it is necessary to use a liquid crystal material or form a complex concave-convex pattern, which causes a problem of reduced transmittance and reduced quality of the obtained information.
[0017] In addition, it is recorded that in the film described in patent document 4, the phase difference is controlled at a low level, and in the film described in patent document 5, the phase difference is controlled at a high level, thereby suppressing the color unevenness when used for liquid crystal display devices. However, not only there is no opinion on the elimination of color unevenness when used as a back panel, but also there are problems of heat resistance and bending resistance. In particular, the film described in patent document 4 is fragile, and the film described in patent document 5 makes anisotropy stronger in order to improve the phase difference, and the operation is difficult. In addition, due to the thick film thickness, there are problems in bending resistance.
[0018] Therefore, the present invention aims to provide an image display device that can eliminate the above-mentioned color unevenness without using a depolarizing member, thereby achieving excellent image quality even for a photoelectric conversion element such as a camera arranged on the side opposite to the viewer side of an array of light-emitting elements for image display. In addition, it is preferable to provide an image display device for a flexible image display device.
[0019] Means for solving problems
[0020] The gist of the present invention for solving the above-mentioned problems is as follows.
[0021] That is, as follows.
[0022] [1] A film for a back panel, which is a film for a back panel of an image display device, wherein the image display device is equipped with a polarizing plate, an array of light-emitting elements for image display, a back panel, and a photoelectric conversion element in sequence when viewed from a viewer's side, wherein the phase difference value of the back panel film is greater than 0 nm and less than 1000 nm, and the phase difference value is obtained by causing light with a wavelength of 590 nm to be incident at an incident angle of 40° along a plane including a fast axis of the film and a perpendicular axis relative to the film surface, with the perpendicular axis being a reference of 0°.
[0023] [2] The back sheet film according to [1], comprising a biaxially oriented polyester film as one of its components.
[0024] [3] According to the back panel film described in [2], the biaxially oriented polyester film is a single-layer film or a film formed by stacking multiple layers, and has at least one polyester resin layer, wherein the polyester resin layer contains 6 mol % or more of isophthalic acid components in all dicarboxylic acid components of the polyester resin constituting the layer.
[0025] [4] According to the back panel film described in [2] above, the polyester constituting the biaxially oriented polyester film is a polyester obtained by polymerization or copolymerization of at least one selected from naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, fluorene derivatives, terephthalic acid, bisphenol A, isosorbide, cyclohexanedimethanol and their ester-forming derivatives, or a polyester containing polyetherimide.
[0026] [5] The back sheet film according to [2] above, wherein the crystallinity is 30% or less and the rigid amorphous content is 20% or more and 50% or less.
[0027] [6] The back panel film according to [1] is a film formed by stacking two or more layers, and when the thickness direction refractive index of the layer with the largest thickness direction refractive index is set to nA and the thickness direction refractive index of the layer with the smallest thickness direction refractive index is set to nB, the following formula (1) is satisfied.
[0028] nA-nB ≥ 0.02 (1)
[0029] [7] The back sheet film according to [1], wherein the increase in haze (Δhaze) when heat treated at 120° C. for 5 hours is 0% or more and 2.0% or less.
[0030] [8] The back sheet film according to [2], wherein the relaxation time of the movable amorphous phase of the biaxially oriented polyester film after heat treatment at 120° C. for 3 minutes in TD-NMR measurement is 0.200 ms or less.
[0031] [9] The back panel film according to [2], wherein in the Fourier transform infrared spectroscopy (FT-IR) spectrum of the thickest layer among the layers constituting the film, the -1 The spectral intensity r2 observed at 1388 cm -1 The ratio R(r2 / r1) of the spectral intensity r1 observed at location satisfies the following formula (2).
[0032] 1.0 < R < 1.8 (2)
[0033]
[10] The back sheet film according to [1], wherein the flexural rigidity is 0.2 mN or more and 20.0 mN or less in both the longitudinal direction and the width direction.
[0034]
[11] According to the back panel film described in [2], the amorphous density A of the biaxially oriented polyester film is greater than 1.0, and the amorphous density A is calculated by ΔHg / ΔCp, wherein ΔHg / ΔCp is obtained by dividing the endothermic amount ΔHg observed in the irreversible curve of temperature-modulated DSC (30-150°C) by the specific heat capacity difference ΔCp before and after the glass transition temperature observed in the reversible curve.
[0035]
[12] The back panel film according to [1], wherein the angle of restoration is 140° or more in both the longitudinal direction and the width direction.
[0036]
[13] The back sheet film according to [1], wherein the elongation at break is 50% or more in both the longitudinal direction and the width direction.
[0037]
[14] The back panel film according to [1], wherein the number of times the film is bent to break as evaluated using an MIT bending tester is 1,000 times or more in both the longitudinal direction and the width direction.
[0038]
[15] The back panel film according to [1], wherein the difference between the average transmittance of P waves when p-polarized light is incident at an incident angle of 40° and the average transmittance of S waves when s-polarized light is incident at an incident angle of 40° is 10% or less.
[0039]
[16] A polyester film, which is a polyester film made of a dicarboxylic acid component and a diol component, wherein the terephthalic acid component in the dicarboxylic acid component is 50 mol% or more and 95 mol% or less, and the ethylene glycol component in the diol component is 50 mol% or more and 95 mol% or less, the melting point observed on the lowest temperature side is 240°C or less, the density is 1.360 g / cc or less, and the phase difference value obtained by making light with a wavelength of 590 nm incident at an incident angle of 40° with the vertical axis as a reference 0° along a plane including the fast axis of the film and the vertical axis relative to the film surface is 0 nm or more and 1000 nm or less.
[0040]
[17] The polyester film according to
[16] , wherein the polyester film is a single-layer film or a film formed by stacking a plurality of layers, and has at least one polyester resin layer, wherein the polyester resin layer contains 6 mol % or more of isophthalic acid components in the total dicarboxylic acid components of the polyester resin constituting the layer.
[0041]
[18] The polyester film according to
[16] , wherein the polyester constituting the polyester film is a polyester obtained by polymerizing or copolymerizing at least one selected from naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, fluorene derivatives, terephthalic acid, bisphenol A, isosorbide, cyclohexanedimethanol and their ester-forming derivatives, or a polyester containing polyetherimide.
[0042]
[19] The polyester film according to
[16] , wherein the degree of crystallinity is 30% or less and the amount of rigid amorphous particles is 20% or more and 50% or less.
[0043]
[20] The polyester film according to
[16] , wherein the relaxation time of the movable amorphous phase in TD-NMR measurement after heat treatment at 120° C. for 3 minutes is 0.200 ms or less.
[0044]
[21] The polyester film according to
[16] , wherein in the Fourier transform infrared spectroscopy (FT-IR) spectrum of the thickest layer among the layers constituting the film, the -1 The spectral intensity r2 observed at 1388 cm -1 The ratio R(r2 / r1) of the spectral intensity r1 observed at location satisfies the following formula (2).
[0045] 1.0 < R < 1.8 (2)
[0046]
[22] The polyester film according to
[16] , wherein the bending rigidity is 0.2 mN or more and 20.0 mN or less in both the longitudinal direction and the width direction.
[0047]
[23] The polyester film according to
[16] has an amorphous density A of greater than 1.0, and the amorphous density A is calculated by ΔHg / ΔCp, wherein ΔHg / ΔCp is obtained by dividing the endothermic amount ΔHg observed in the irreversible curve of temperature-modulated DSC (30 to 150°C) by the specific heat difference ΔCp before and after the glass transition temperature observed in the reversible curve.
[0048]
[24] The polyester film according to
[16] , wherein the elongation at break is 50% or more in both the longitudinal direction and the width direction.
[0049]
[25] An image display device comprising the back panel film described in [1] or the polyester film described in
[16] .
[0050]
[26] The image display device according to
[25] , wherein the light-emitting element array for an image display device used in the image display device is an organic electroluminescent element array.
[0051]
[27] According to the image display device described in
[25] , the angle range in which the photoelectric conversion element mounted on the image display device can receive light is greater than 60° and less than 140°.
[0052]
[28] A foldable display equipped with the back panel film described in [1] or the polyester film described in
[16] .
[0053]
[29] A device having an image display device as one of its components, wherein the image display device is equipped with the back panel film described in [1] or the polyester film described in
[16] .
[0054] Effects of the Invention
[0055] According to the present invention, by using the film for the back panel of the present invention, a flexible image display device can be provided, wherein even a photoelectric conversion element such as a camera arranged on the side opposite to the viewer side of the image display light-emitting element array can suppress the generation of rainbow spots, and the shooting quality is excellent. In addition, a polyester film can be provided, which can suppress the generation of rainbow spots when used in an optical device such as an image display device. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 This is a schematic front view of an example of an image display device of the present invention.
[0057] Figure 2 Reference diagram for explaining the R40 measurement test
[0058] Figure 3 Reference diagram for understanding the bending rigidity measurement test
[0059] Figure 4 This figure explains the structure of the device used in the visibility test.
[0060] Figure 5 Reference diagram for understanding the test of measuring the angle of recovery DETAILED DESCRIPTION
[0061] The image display device using the back panel film of the present invention is equipped with a polarizing plate, an array of light-emitting elements for image display, a back panel, and a photoelectric conversion element in order from the viewer side (the side displaying the image. Hereinafter, it is sometimes referred to as the "front side"). In such an image display device, components other than these components may also be mounted. For example, an adhesive layer may be provided between the array of light-emitting elements for image display and the back panel. In addition, a color filter, a lens film, a diffuser, an anti-reflection film, etc. may be provided as needed. In addition, hereinafter, the side opposite to the viewer side (the side not displaying the image) is sometimes referred to as the back side.
[0062] In the image display device using the back panel film of the present invention, a polarizing plate is arranged on the front side when viewed from the image display light emitting element array in order to prevent the visibility of the displayed image and the contrast ratio from being reduced due to light entering the display device from the outside.
[0063] As for the polarizing plate used in the present invention, by being used as a circular polarizing plate used together with an optical film (λ / 4 phase difference film) and applied to an organic electroluminescent display device, etc., it can shield the reflected light from the metal electrode of the organic electroluminescent element and the like in the full wavelength of visible light, and can prevent reflection during observation, and can improve the black presentation. The circular polarizing plate is composed of a polarizer that converts incident light into linear polarized light, and a phase difference plate that converts linear polarized light into circularly polarized light.
[0064] The polarizing plate can be selected and used appropriately from any polarizing plate or coated polarizing film used in the field related to the image display device. As a representative polarizing plate, a polarizing plate obtained by dyeing a dichroic material such as iodine on a polyvinyl alcohol film or the like can be cited, but the present invention is not limited thereto, and a known polarizing plate or a polarizing plate that may be developed in the future can be selected and used appropriately.
[0065] The phase difference plate can be appropriately selected and used in the field related to the image display device. As the phase difference plate, a phase difference plate obtained by stretching a plastic film in a specific direction can be used, and polycarbonate, polyester, polysulfone, polystyrene, polymethyl methacrylate, etc. can be cited. It should be noted that the phase difference plate can be formed using a layer of birefringent film, but it can also be formed by stacking multiple birefringent films in a manner that reduces the wavelength dependence of the phase difference value and functions in the entire visible light wavelength region.
[0066] The polarizer and the phase difference plate can be bonded together using an acrylic transparent adhesive or pressure-sensitive adhesive that does not have optical anisotropy.
[0067] It should be noted that, from the viewpoint of preventing the visibility from being reduced due to the reflection of external light on its surface, an anti-reflection film may be provided on the surface of the polarizing plate. For example, in addition to directly forming a multilayer film on the surface of the polarizing plate, an anti-reflection film may also be attached. In addition, a material with a microstructure such as a moth-eye structure may be provided, and an appropriate anti-glare treatment may be further implemented.
[0068] As one of the components of the image display device using the back panel film of the present invention, the image display light emitting element array can be appropriately selected and used in any image display light emitting element array used in the field related to the image display device. As a representative image display light emitting element array, a light emitting element array using organic electroluminescent elements, a light emitting element array using inorganic electroluminescent elements, and a light emitting element array using organic light emitting diodes and micro light emitting diodes can be cited, but it is not limited to this, and the image display light emitting element array known and possibly developed in the future can be appropriately selected and used. Among them, in order to achieve high contrast and form a clear image, it is preferred to use an organic electroluminescent element.
[0069] As the light-emitting element array for image display, an organic electroluminescent element array can be suitably used. As an example of an organic electroluminescent element array, it includes a substrate, a thin film transistor, an organic electroluminescent element and a sealing layer, and the organic electroluminescent element includes an anode, a light-emitting layer and a cathode. For example, it can have the following layer structures (i) to (vi). In addition, the following light-emitting layer can be a light-emitting layer composed of a blue light-emitting layer, a green light-emitting layer and a red light-emitting layer.
[0070] Representative examples of the structure of the organic electroluminescent element are shown below.
[0071] (i) Anode / Hole injection and transport layer / Emitting layer / Electron injection and transport layer / Cathode
[0072] (ii) Anode / hole injection and transport layer / light-emitting layer / hole blocking layer / electron injection and transport layer / cathode
[0073] (iii) anode / hole injection and transport layer / electron blocking layer / light-emitting layer / hole blocking layer / electron injection and transport layer / cathode
[0074] (iv) Anode / hole injection layer / hole transport layer / light-emitting layer / electron transport layer / electron injection layer / cathode
[0075] (v) Anode / hole injection layer / hole transport layer / light-emitting layer / hole blocking layer / electron transport layer / electron injection layer / cathode
[0076] (vi) anode / hole injection layer / hole transport layer / electron blocking layer / light-emitting layer / hole blocking layer / electron transport layer / electron injection layer / cathode.
[0077] The substrate is a member for supporting various elements of the array of light-emitting elements for image display, and can be formed by an insulating material. The back panel film of the present invention can be suitably used as this substrate. If this substrate is thin and has weak rigidity, it will sag when various elements are configured. This back panel film supports the array of light-emitting elements for image display in a manner that does not sag, and plays a role in protecting the array of light-emitting elements for image display from moisture, heat, impact, etc. In order to bond the array of light-emitting elements for image display to the back panel film, an adhesive layer can be configured between the array of light-emitting elements for image display and the back panel film.
[0078] The phase difference value (hereinafter sometimes referred to as "R40") of the back panel film of the present invention is greater than 0nm and less than 1000nm, and the phase difference value is obtained by incident light of a wavelength of 590nm at an incident angle of 40° with the vertical axis as a reference 0° along a plane including the fast axis of the film and the vertical axis relative to the film surface. By controlling R40 within the above range, the accuracy of the information obtained by the photoelectric conversion element is high, for example, the color unevenness of an image taken by a camera can be reduced, and the recognition accuracy of the sensor is improved. The smaller R40 is, the higher the accuracy of the information obtained by the photoelectric conversion element, and R40 is preferably less than 800nm, and more preferably less than 500nm. It should be noted that in the present invention, R40 is obtained by the method described in (4) front phase difference Re, R40 described later.
[0079] As a method for controlling R40 within a range of more than 0nm and less than 1000nm, the birefringence in the thickness direction of the film and the film is controlled. In particular, the phase difference of the unstretched film of the amorphous resin is small, so the method generally adopted is to use an amorphous resin. Here, the so-called amorphous resin refers to a resin having a crystalline melting enthalpy (hereinafter also referred to as "ΔHm") less than 5J / g obtained by a differential scanning calorimeter (hereinafter also referred to as "DSC"). As an example of a representative amorphous resin for optical purposes, cyclic olefin resins, polystyrene resins, polycarbonate resins, acrylic resins, cellulose triacetate, and copolyesters are often used from the viewpoint of optical quality. In particular, from the viewpoint of heat resistance and productivity, bicyclo〔2,2,1〕hept-2-ene (hereinafter referred to as norbornene), tricyclo〔4,3,0,12.5〕dec-3-ene and other tricyclic olefins with 10 carbon atoms (hereinafter referred to as tricyclodecene), tetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene and other tetracyclic olefins with 12 carbon atoms (hereinafter referred to as tetracyclododecene), cyclopentadiene, or 1,3-cyclohexadiene are widely used as cyclic olefin resins. In addition, the film thickness can be made thinner as long as the supporting function is not impaired. In addition, the so-called crystalline resin refers to a resin with a ΔHm of 5 J / g or more.
[0080] In addition, from the viewpoint of being able to cope with the foldable display described later, the back panel film of the present invention is preferably a polyester film oriented along a biaxial direction. If it is a polyester film oriented along a biaxial direction, the Young's modulus and elongation at break described later can be controlled by appropriately setting the stretching conditions. In addition, by making it biaxially oriented, the uneven thickness of the film is reduced, and a high-quality film can be obtained. It should be noted that the so-called biaxially oriented film in the present invention refers to the following film: with respect to the refractive index nx, ny, and nz of more than one layer constituting the film (here, the refractive index in the length direction is set to nx, the refractive index in the width direction is set to ny, and the refractive index in the thickness direction is set to nz), the average value of nx, ny and nz is smaller than nx, ny and larger than nz. However, it is usually carried out by orienting along the biaxial direction and plane orientation, and R40 becomes larger, so it is necessary to thin the film or pass through the resin composition and film-making process described later, thereby controlling the higher-order structure of the film within the range that does not hinder the purpose of the present invention.
[0081] In addition, the so-called polyester film in the present invention refers to a film in which polyester is used as the main component as the resin constituting the film, and the so-called polyester in the present invention is a polymer obtained by a dicarboxylic acid constituent component and a diol constituent component or their ester-forming derivatives. It should be noted that in the present invention, the so-called constituent component represents the smallest unit obtainable by hydrolyzing the polyester. In addition, the so-called main component refers to the resin with the largest content in the resin constituting the film, and when the total mass of the resin constituting the film is set to 100 mass%, the resin is preferably contained in the film in an amount greater than 50 mass%, more preferably 70 mass% or more. In addition, as long as it does not hinder the purpose of the present invention, a part of oxyacids such as hydroxybenzoic acid may also be used.
[0082] Examples of the dicarboxylic acid constituent component constituting the polyester used in the present invention include terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,2-cyclohexane dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, 9,9-bis(carboxymethyl)fluorene, 9,9-bis[2-carboxyethyl]fluorene, 9,9-bis[1-carboxyethyl]fluorene, 9,9-bis[2-carboxy-1-cyclohexylethyl]fluorene, 9,9-bis[2-carboxy-1-phenylethyl]fluorene, 4,4'-diphenyl dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, sodium isophthalic acid-5-sulfonate, phenyl indan dicarboxylic acid, anthracene dicarboxylic acid, phenanthrene dicarboxylic acid, 9,9'-bis (4-carboxylphenyl) fluorene acid and other aromatic dicarboxylic acids, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, dimer acid, eicosanedioic acid, pimelic acid, azelaic acid, methylmalonic acid, ethylmalonic acid and other aliphatic dicarboxylic acids, adamantane dicarboxylic acid, norbornene dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, decalin dicarboxylic acid and other alicyclic dicarboxylic acids. Among them, preferably aromatic dicarboxylic acids are used as the main dicarboxylic acid constituents. These dicarboxylic acid constituents can use only one kind, or two or more kinds can be used in combination. Among them, it is preferred to use at least one selected from naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, 9,9-bis[2-carboxyethyl]fluorene, 9,9-bis[1-carboxyethyl]fluorene, 9,9-bis[2-carboxy-1-cyclohexylethyl]fluorene, and 9,9-bis[2-carboxy-1-phenylethyl]fluorene.
[0083] Examples of the diol constituent component constituting the polyester used in the present invention include ethylene glycol, 1,3-butanediol, 1,4-butanediol, tetramethylene glycol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, terephthalylidene alcohol, diethylene glycol, triethylene glycol, polyalkylene glycol, isosorbide, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,5-pentanediol, 1,7-heptanediol, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-methylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3,5-dimethylphenyl]fluorene, 2,2-bis(4-hydroxyethoxyphenyl)propane, bisphenol A, and spirodiol. These diol constituent components may be used alone or in combination of two or more. Among them, it is preferred to use at least one component selected from the group consisting of terephthalic acid, bisphenol A, isosorbide, cyclohexanedimethanol, 9,9-bis(tert-butoxycarbonylmethyl)fluorene, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-methylphenyl]fluorene, and 9,9-bis[4-(2-hydroxyethoxy)-3,5-dimethylphenyl]fluorene.
[0084] In particular, when the sum of all dicarboxylic acid components and diol components is set to 100 mol%, it is more preferred that the total amount of naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, the above-exemplified fluorene derivatives, terephthalic acid, bisphenol A, isosorbide, and cyclohexanedimethanol is preferably 5 mol% or more, and more preferably 7.5 mol% or more. By making such a copolymerized polyester, the amorphous property of the polyester is improved, and the value of R40 can be controlled at a low level. In addition, since the proportion of the amorphous structure increases, the amount of the above-mentioned agglomerated amorphous component can be increased, and the value of ΔHg representing the amount of agglomerated amorphous can be easily controlled at a high level. From the viewpoint of improving amorphous property, it is further preferred to use two of these copolymer components. In addition, the glass transition temperature Tg can be increased, and even at the processing temperature when incorporated into the image display device, the increase in haze can be suppressed, and a film with excellent transparency can be obtained.
[0085] In addition, the polyester may contain resins other than polyester, and polyetherimide may be cited as such a resin. By containing polyetherimide, the ratio of the above-mentioned amorphous structure can be increased, and the value of R40 can be controlled at a low level. In addition, by increasing the ratio of the amorphous structure, the amount of agglomerated amorphous components can be increased.
[0086] The recovery angle of the back panel film of the present invention is preferably 140° or more in both the length direction and the width direction, and more preferably 160° or more. The recovery angle can be evaluated by the measurement method shown in (18) bending resistance described later. By controlling the recovery angle within this range, even if the image display device is repeatedly folded or unfolded several times, the generation of wrinkles and floating phenomena when used as a back panel film can be more significantly suppressed.
[0087] In order to control the recovery angle within the above range, the bending rigidity of the film is preferably less than 20.0mN in the length direction and the width direction, and more preferably less than 10.0mN. In addition, by making the bending rigidity more than 0.2mN, it becomes possible to support with a margin in a manner that does not cause the image display light-emitting element array to sag. From the viewpoint of support, the bending rigidity is more preferably set to more than 1.0mN. There is no particular restriction on the method of controlling the bending rigidity within this range, but it is most effective to control the thickness of the film, and the thickness of the film is preferably set to more than 10μm and less than 70μm, and more preferably set to more than 10μm and less than 50μm. On this basis, in order to control the bending rigidity at a low level, the main method adopted is to reduce the Young's modulus, and the Young's modulus in the length direction and the width direction is preferably more than 1.5GPa and less than 4.5GPa, preferably set to more than 2.0GPa and less than 4.0GPa. As a method for controlling the Young's modulus, a resin with a high Young's modulus such as a polyester resin will also become larger. In addition, among polyester resins, if the non-crystalline property is improved by including copolymer components, the Young's modulus can be reduced. In addition, the Young's modulus is related to the oriented crystal state of the film, and can also be controlled by stretching ratio, stretching temperature, heat treatment temperature, heat shrinkage treatment, etc. For example, if the stretching ratio in one direction is increased and the stretching ratio in the other direction is reduced, the Young's modulus in the high ratio direction is higher, and the Young's modulus in the low ratio direction is lower. Therefore, in order to make the Young's modulus below 4.0GPa, the stretching ratio can be made more than 2 times and less than 4.5 times in both the length direction and the width direction, thereby controlling the Young's modulus within the above range. In addition, if the orientation state of the film is relaxed, there is a tendency for the Young's modulus to decrease. Therefore, in order to make the Young's modulus above 2.0GPa, it is necessary to use the melting point of the layer with the lowest melting point among the resins constituting the film as a reference and heat-treat below the melting point + 10°C. For example, when the copolyester having a melting point of 226° C. is the layer with the lowest melting point, the heat treatment temperature is preferably 226° C. to 236° C. In addition, a plasticizer or an elastomer may be added to reduce the Young's modulus as long as the effect of the present invention is not impaired.
[0088] The film for the back panel in the present invention is preferably a polyester film, more preferably a polyester film oriented along a biaxial direction. In this case, ΔHg / ΔCp (hereinafter also referred to as "amorphous density A") is preferably greater than 1.0, and the ΔHg / ΔCp is obtained by dividing the endothermic value ΔHg (unit: J / g) observed between 30°C and 150°C in the irreversible curve of temperature-modulated differential scanning calorimetry (temperature-modulated DSC) by the specific heat difference ΔCp (unit: J / (g°C)) before and after the glass transition temperature observed between 30°C and 150°C in the reversible curve.
[0089] By controlling the amorphous density A within the above range, the bending resistance can also be improved, and the recovery angle can be controlled at a high level. As a preferred range, ΔHg / ΔCp is preferably greater than 1.0 and less than 10.0, and as a lower limit, it is more preferably greater than 2.0, particularly preferably greater than 2.5, and as an upper limit, it is more preferably less than 7.0. The reason why the bending resistance can be improved by controlling the amorphous density is as follows.
[0090] The polyester film is composed of polymer chains, and therefore contains a crystalline component with high rigidity, a rigid amorphous component, and a movable amorphous component. Due to its heterogeneity, the movable amorphous component includes an agglomerated amorphous component in which the polymer chains are relatively agglomerated and rigid, and a relaxed amorphous component in which the polymer chains are dispersed. The amount of relaxed amorphous component in the polyester film can be obtained by subtracting the amount of agglomerated amorphous component from the amount of movable amorphous component according to the above relationship. The amount of movable amorphous component and the amount of agglomerated amorphous component can be analyzed using temperature-modulated DSC. The specific heat difference ΔCp before and after the glass transition temperature observed between 30°C and 150°C in the reversible curve obtained by temperature-modulated DSC is proportional to the amount of movable amorphous component. In addition, the endothermic heat ΔHg observed between 30°C and 150°C in the irreversible curve is the heat required for the agglomerated amorphous component to relax and transform into the relaxed amorphous component, and therefore depends on the amount of agglomerated amorphous component. In addition, the values of ΔCp and ΔHg can be obtained as the average value of three measurements.
[0091] The method of controlling ΔHg / ΔCp within the above range is described in, for example, the following steps (1) and (2), and can be controlled particularly by the temperature in the third stage of the heat treatment step and the relaxation rates in the longitudinal and transverse directions.
[0092] Step (1) Step of stretching the film to 3.7 to 4.5 times in the transverse stretching direction
[0093] Step (2) A step of performing a heat treatment relaxation at a temperature of 210°C or higher and 245°C or lower
[0094] In addition, each step is described in detail below.
[0095] Regarding step (1): a step of stretching to 3.7 times or more and 4.5 times or less in the transverse stretching direction, in order to obtain the effect of the present invention, it is important to perform stretching in three stages, and further, the stretching ratios in the first stage, the second stage, and the third stage preferably satisfy the following conditions.
[0096] Stage 1: 2.0 times or more and less than 2.5 times
[0097] Stage 2: ≤1.5 times
[0098] Stage 3: ≤1.5 times.
[0099] Regarding process (2): a process of heat treatment relaxation at a temperature above 220°C and below 245°C. In order to obtain a more significant effect of the present invention, it is important to carry out the heat treatment relaxation in three stages. Furthermore, the heat treatment temperatures of the first stage, the second stage and the third stage and the longitudinal and transverse relaxation rates preferably satisfy the following conditions.
[0100] Stage 1: 150°C or higher and 245°C or lower
[0101] Stage 2: 220°C or higher and 245°C or lower
[0102] Stage 3: 100°C or higher and 180°C or lower
[0103] Longitudinal relaxation rate: 1% or more and 8% or less
[0104] Transverse relaxation rate: 1% or more and 8% or less.
[0105] As the reason why the bending resistance is improved by increasing the value of ΔHg / ΔCp, the following can be considered. The polyester film is composed of polymer chains, and therefore contains a crystalline component with higher rigidity, a rigid amorphous component, and a movable amorphous component. The movable amorphous component has agglomerated amorphous components with rigidity due to its heterogeneity, and a relaxed amorphous component formed by the dispersion of polymer chains. It is believed that when the polyester film is bent, in its bent portion, the forces of extension and compression are applied to the polymer chains, and the relaxed amorphous components with lower rigidity undergo plastic deformation. The polyester film undergoes plastic deformation under the action of bending, and thus, when it is left to stand for a certain period of time in a folded state, plastic deformation occurs, and wrinkles, floating, cracks, etc. are generated in the polyester film. In addition, for repeated bending, the base point of the break of the polyester film is generated due to plastic deformation, resulting in breakage. Based on the above content, it is believed that in order to make the static bending resistance good, it is preferable to increase the agglomerated amorphous components and reduce the amount of relaxed amorphous components. That is, it is believed that by increasing ΔHg indicating the amount of aggregated amorphous components and decreasing ΔCp indicating the amount of movable amorphous components, that is, the value of ΔHg / ΔCp is large, the bending resistance becomes good. It should be noted that ΔHg and ΔCp can be obtained by the method described in the item of ΔCp, ΔHg, and rigid amorphous component Xra of the film (12).
[0106] The image display device using the back panel film of the present invention is preferably flexible, preferably a foldable display with a bendable curved portion with a bending diameter of more than 1mm and less than 10mm. The so-called foldable display is a display that can be folded into two folds when carried. The more preferred range of the bending diameter is 8mm or less as the upper limit, more preferably 6mm or less, and more preferably 5mm or less. If the bending diameter is less than 10mm, thinning in the folded state can be achieved. It can be said that the smaller the bending diameter, the better, but the smaller the bending diameter, the easier it is to produce creases. The bending diameter is preferably more than 0.1mm, and can also be more than 1mm. Even if the bending diameter is 1mm, it is possible to achieve a thinness that is practical enough when carried. In addition, the foldable display can be three-fold, four-fold, and in addition, it can also be a winding type that is considered to be reelable, and they all fall within the scope of the so-called foldable display in the present invention.
[0107] The elongation at break of the back panel film of the present invention is preferably 50% or more in both the length direction and the width direction. By making the elongation at break 50% or more, the number of times the bending obtained by evaluation using the MIT bending tester reaches the break can be more than 1000 times in the length direction and the width direction, and when it is installed on a foldable display and repeatedly bent, the film fatigue and break can be suppressed. When the elongation at break is 100% or more, it is more preferred from the viewpoint of suppressing the break when repeated bending is performed. It should be noted that the higher the elongation at break, the more preferred it is. Therefore, as an upper limit, there is no particular restriction, but as long as it is less than 300% in both the length direction and the width direction, it is sufficient. In order to improve the elongation at break, it can be achieved by giving entanglement and orientation of molecular chains in at least one layer of the layer structure of the film constituting the back panel film and in the higher-order structure of the film. A particularly effective method is to include a crystalline polyester resin as a resin. In addition, the ΔHm of the crystalline polyester resin is more preferably 25 J / g or more. In order to increase the density of entanglement points, it can be achieved by making the molecular weight of the crystalline resin high, that is, increasing the intrinsic viscosity (also called "IV") of the film. As a preferred IV, it is 0.60 or more and less than 1.00. However, if it is above 1.00, it is necessary to use a resin with high viscosity to achieve it, which is difficult to melt extrude. If it is less than 0.60, it is difficult to form entanglement points and difficult to impart orientation by stretching. It is preferably 0.65 or more and less than 0.90, and most preferably 0.68 or more and less than 0.85. From the viewpoint of making the IV when the film is made into the above range, the IV of the resin used is preferably 0.65 or more and less than 1.00, more preferably 0.70 or more and less than 0.90, and most preferably 0.80 or more and less than 0.90. In addition, from the viewpoint of imparting orientation, the stretching ratios in the length direction and the width direction are preferably 3 times or more and 5 times or less. It should be noted that the higher the number of times the above-mentioned bending reaches the break, the more preferred it is. Therefore, as an upper limit, there is no particular restriction, and it is sufficient to be less than 100,000 times.
[0108] The increase in haze (Δ haze) of the back panel film of the present invention when subjected to a heat treatment for 5 hours at 120°C is preferably 2.0% or less. By controlling the Δ haze within the above range, even if the back panel film is subjected to a heat-applied process in the processing of the image display device using the back panel film, whitening will not occur, and the visibility of the image display device can be maintained at a high level. From the perspective of maintaining visibility at a high level, the Δ haze is preferably less than 2.0%, more preferably less than 1.5%, further preferably less than 1.0%, and most preferably less than 0.5%. It should be noted that the lower limit of the Δ haze is zero. The so-called processing here refers to the process applied until the functional layer is formed on the back panel film and the product is manufactured. For example, the processing of applying an adhesive, the processing of forming a hard coating layer, the processing of vapor-depositing a transparent conductive layer, the lamination processing of bonding the films to each other, and the annealing processing can be cited.
[0109] As a countermeasure for suppressing Δ haze, it is possible to cite the method of controlling the heat of thermal crystallization ΔHc obtained by DSC at a low level. ΔHc is preferably set to less than 15 J / g, more preferably set to less than 10 J / g, and most preferably set to less than 7 J / g. The reason for the increase in haze during heat treatment is mainly due to the thermal crystallization of the movable amorphous component into the crystalline component caused by the application of heat. By controlling ΔHc at a low level, the proportion of the movable amorphous amount that can be thermally crystallized is reduced, and it becomes less likely to whiten due to heat treatment. Therefore, the Δ haze can be controlled to be smaller. As a method of reducing ΔHc, an amorphous resin such as COP that is not thermally crystallized is used to form an alloy state that hinders thermal crystallization. Alternatively, on the basis of using a crystalline resin, it is necessary to form a higher-order structure of the film based on oriented crystallization within a range that does not impair the effect of the present invention. From the viewpoint of controlling ΔHc within the above range, the heat treatment temperature when the film is heat treated is preferably below the melting point + 7°C based on the melting point of the resin constituting the layer with the lowest melting point among the layers constituting the film, and more preferably below the melting point + 5°C based on the melting point of the resin constituting the layer with the lowest melting point. As described above, from the viewpoint of reducing the movable amorphous component, it is preferred that the rigid amorphous amount is 20% or more. As the upper limit of the rigid amorphous amount, from the viewpoint of reducing R40 as described later, it is 50% or less. It should be noted that the rigid amorphous amount can be obtained by the method described in the items (11) ΔCp, ΔHg, and rigid amorphous amount Xra of the film.
[0110] In addition, from the viewpoint of suppressing the Δ haze within the above range, the relaxation time of the movable amorphous phase in the TD-NMR (Time domain NMR) measurement after a heat treatment at 120°C for 3 minutes is preferably 0.200ms or less. In this measurement, the molecular mobility of the movable amorphous component at 120°C is evaluated. The faster the relaxation time, the lower the molecular mobility and the more difficult it is to perform thermal crystallization. As described above, the increase in haze can be suppressed not only by reducing the amount of the above-mentioned movable amorphous component, but also by slowing down the thermal crystallization of the movable amorphous component. As a method for controlling the relaxation time of the movable amorphous phase in the TD-NMR measurement within the above range, it is preferred to set the IV of the film to be greater than 0.65, and it is more preferred to set the IV of the film to be greater than 0.68. By achieving a high IV, the molecular mobility can be controlled at a low level, thereby controlling the relaxation time of the movable amorphous amount at a low level. It should be noted that the lower limit of the relaxation time of the movable amorphous phase is not particularly limited, but is practically 0.100 ms or less.
[0111] With regard to the film for the back panel of the present invention, it is preferred that a laminated film is made by stacking more than two layers, and when the refractive index in the thickness direction of the layer with the largest refractive index in the thickness direction (this layer is referred to as "layer A") is set to nA, and the refractive index in the thickness direction of the layer with the smallest refractive index in the thickness direction (this layer is referred to as "layer B") is set to nB, the following formula (1) is satisfied.
[0112] nA-nB≥0.02(1).
[0113] By controlling the refractive index of each layer of the film in a manner satisfying formula (1), the mechanical strength of the film can be improved by having a layer B with a small refractive index in the thickness direction, and the elongation at break can be controlled within the above range. The higher nA-nB is, the more preferred it is, but it is practically 0.15 or less. In addition, by having a layer A with a large refractive index in the thickness direction, the phase difference in the thickness direction can be controlled at a low level, and R40 can be controlled within the above preferred range. By setting the composition in which the refractive index of each layer is controlled in this way, it is possible to achieve a balance between optical properties and mechanical properties. It should be noted that, from the viewpoint of controlling R40 at a low level, the smaller the sum of the thickness of the layers having the same refractive index as layer B, the more preferred it is. On the other hand, from the viewpoint of performing stable film formation, the sum of the thickness of the layers having the same refractive index as layer B is preferably larger. Due to the above reasons, the sum of the thickness of the layers having the same refractive index as layer B is preferably greater than 4 μm and less than 10 μm.
[0114] As a method for controlling in a manner that satisfies formula (1), it can be achieved as follows: when the melting point of the resin constituting layer A is set to TmA and the melting point of the resin constituting layer B is set to TmB, TmA>TmB is set, and heat treatment is performed at a heat treatment temperature of more than TmB-15°C and less than TmA-5°C. It should be noted that, with respect to the heat treatment temperature, there is a tendency that the higher the temperature, the more the orientation is relaxed and the R40 is reduced, but if the heat treatment is performed at a heat treatment temperature higher than TmA-5°C, the film sometimes melts and film formation cannot be performed. There is no limitation on the method for controlling the melting point of the constituent resin, but it is preferably a method of controlling by adding a copolymer component. For example, by copolymerizing isophthalic acid in a dicarboxylic acid component, the melting point can be lowered compared to the case where no copolymerization occurs, and a melting point difference can be given to the resin constituting layer A and the resin constituting layer B.
[0115] From the viewpoint of being able to easily ensure a melting point difference, it is preferred to have at least one polyester resin layer containing 6 mol % or more of an isophthalic acid component in all dicarboxylic acid components constituting the polyester resin.
[0116] In addition, the polyester film used in the present invention preferably uses the following polyester resin in at least one layer constituting the layer of the film, wherein the terephthalic acid component in the dicarboxylic acid component is 50 mol% or more and 95 mol% or less, and the ethylene glycol component in the diol component is 50 mol% or more and 95 mol% or less. In addition, from the viewpoint of easing orientation, the melting point on the lowest temperature side measured by DSC is more preferably 240°C or less. The melting point on the lowest temperature side measured by DSC is further preferably 230°C or less. As the lower limit, there is no particular restriction, but it is preferably set to 200°C or more.
[0117] In addition, as a method for reducing the refractive index in the thickness direction, a method of increasing the amorphousness of the resin is generally adopted, and examples thereof include polyester resins obtained by using any of the constituent components selected from naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, the fluorene derivatives exemplified above, terephthalic acid, bisphenol A, isosorbide, cyclohexane dicarboxylic acid, and cyclohexanedimethanol as described above.
[0118] As the density of the polyester film, from the viewpoint of controlling R40 to be smaller, it is preferably set to 1.360 g / cc or less. As the lower limit, there is no particular restriction, but it is preferably set to 1.34 g / cc or more. As a method for making the density below 1.360 g / cc, a method of making a film structure such as that exemplified above and a method of adopting a heat treatment process can be cited.
[0119] In the Fourier transform infrared spectroscopy (FT-IR) spectrum of the thickest layer among the layers constituting the film, at 1372 cm -1 The spectral intensity r2 observed at 1388 cm-1 The ratio R(r2 / r1) of the spectral intensity r1 observed at location r2 preferably satisfies the following formula (2).
[0120] 1.0 <R<1.8(2)。
[0121] In the stereo conformation of the methylene part of polyethylene terephthalate, it is known that there are two types of structures, namely, the twisted structure and the trans-type structure. Among these two structures, the trans-type structure is advantageous compared with the twisted structure from the perspective of the orderly arrangement of the molecular chains. Therefore, the twisted structure reflects the part where the molecular chains of polyethylene terephthalate are not arranged in order (hereinafter also referred to as the "amorphous part"), and the trans-type structure reflects the structure where the molecular chains of polyethylene terephthalate are arranged in order. In the structure where the molecular chains are arranged in order, there are parts that form a crystal structure (hereinafter also referred to as the "crystalline part") and amorphous parts where the molecular chains are arranged at an intermediate degree between the above-mentioned amorphous part and the crystalline part (hereinafter also referred to as the "oriented amorphous part"), which can be observed by FT-IR. That is, r1 reflects the trans-type structure from the crystalline part, and r2 reflects the twisted structure from the amorphous part. With regard to the crystal structure, due to the molecular orientation, a phase difference is generated, and there is a tendency for the value of R40 to become larger. On the other hand, regarding the amorphous part, since the molecules are oriented in a random direction compared to the crystal structure, there is a tendency that the higher the ratio of the amorphous part, the lower the R40. As shown in formula (2), by making R greater than 1.0, R40 can be controlled at a low level. On the other hand, by making R less than 1.8, Δ haze can be suppressed. In addition, for the same reason, the crystallinity of the film is preferably less than 30%. As a method for controlling the value of R in a manner that satisfies formula (2) and making the crystallinity less than 30%, the following method can be cited: heat treatment is performed at a heat treatment temperature of more than -15°C based on the melting point of the thickest layer of the stacked thickness, and less than +20°C based on the melting point of the thickest layer of the stacked thickness.
[0122] Next, a preferred embodiment of producing the back sheet film of the present invention will be described below, but the present invention is not to be construed as being limited to this embodiment.
[0123] Regarding the most suitable combination of resins of the present invention, the preferred embodiment is as follows: as the resin a constituting the above-mentioned A layer and the resin b constituting the B layer, both resin a and resin b contain 50 mol% or more and 95 mol% or less of terephthalic acid or naphthalene dicarboxylic acid in the acid component, and contain 50 mol% or more and 95 mol% of ethylene glycol in the glycol component. From the viewpoint of controlling R40 below 1000nm, it is particularly preferred to include terephthalic acid as the acid component. In addition, it is preferred to use any monomer of cyclohexanedicarboxylic acid, fluorene derivatives, terephthalic alcohol, bisphenol A, isosorbide, and cyclohexanedimethanol as monomers in both resin a and resin b, and it is more preferred to use any two. By using it in resin a, R40 can be controlled below 1000nm, which is particularly preferred from this point of view. By using it in resin b, the amorphous density A can be controlled at a low level. In addition, by using it in both resin a and resin b, it is also excellent in thermal dimensional stability and heat-resistant reliability tests. In addition, in the resin b, from the viewpoint of lowering the melting point compared with the resin a, it is preferred to use 6 mol % or more of isophthalic acid as the acid component.
[0124] The above-mentioned resin a and resin b are respectively supplied to a venting twin-screw extruder and melt-extruded. At this time, it is preferred that the extruder is in a circulating nitrogen atmosphere, the oxygen concentration is made to be less than 0.7% by volume, and the resin temperature is controlled at 240°C to 320°C. Next, through the filter and the gear pump, the foreign matter is removed and the extrusion amount is uniformed, and a three-layer confluence block with a rectangular lamination portion is used to stack the resin a layer to the surface layer of both sides and the resin b layer to the inner layer, and discharged from the T die in a sheet form onto the cooling drum. At this time, an electrostatic application method in which a high voltage electrode is applied and the cooling drum is made to fit the resin by static electricity, a casting method in which a water film is set between the casting drum and the extruded polymer sheet, a method in which the casting drum temperature is made lower than the glass transition temperature of the polyester resin to make the extruded polymer adhere, or a method in which a plurality of these methods are combined, the sheet polymer is made to fit the casting drum, cooled and solidified, and an unstretched film is obtained. Among these casting methods, when polyester is used, a method of applying static electricity is preferably used from the viewpoint of productivity and planarity.
[0125] From the viewpoints of heat resistance, dimensional stability, mechanical strength, planarity, and uneven thickness, the back panel film of the present invention is preferably stretched in at least one direction. In the case of biaxial orientation, the film can be obtained by stretching the unstretched film in the longitudinal direction and then in the width direction, or by stretching the unstretched film in the width direction and then in the longitudinal direction by a sequential biaxial stretching method, or by stretching the film in the longitudinal direction and the width direction by a biaxial stretching method at about the same time. In addition, the film can be further stretched in the longitudinal direction or the width direction after biaxial orientation.
[0126] In the present invention, after stretching in the longitudinal direction, it is preferred to carry out at least the following steps (1) and (2) in sequence.
[0127] Step (1) Step of stretching the film to 3.7 to 4.5 times in the transverse stretching direction
[0128] Step (2) A step of performing a heat treatment relaxation at a temperature of 210°C or higher and 245°C or lower
[0129] In addition, each step is described in detail below.
[0130] Regarding step (1): a step of stretching to 3.7 times or more and 4.5 times or less in the transverse stretching direction, in order to obtain the effect of the present invention, it is important to perform stretching in three stages, and further, the stretching ratios in the first stage, the second stage, and the third stage preferably satisfy the following conditions.
[0131] Stage 1: 2.0 times or more and less than 2.5 times
[0132] Stage 2: ≤1.5 times
[0133] Stage 3: ≤1.5 times.
[0134] Regarding process (2): a process of heat treatment relaxation at a temperature above 220°C and below 245°C. In order to obtain a more significant effect of the present invention, it is important to carry out the heat treatment relaxation in three stages. Furthermore, the heat treatment temperatures of the first stage, the second stage and the third stage and the longitudinal and transverse relaxation rates preferably satisfy the following conditions.
[0135] Stage 1: 150°C or higher and 245°C or lower
[0136] Stage 2: 220°C or higher and 245°C or lower
[0137] Stage 3: 100°C or higher and 180°C or lower
[0138] Longitudinal relaxation rate: 1% or more and 8% or less
[0139] Transverse relaxation rate: 1% or more and 8% or less.
[0140] It is desirable that the stretching speed in step (1) is 500% / min or more and 100,000% / min or less. In particular, from the viewpoint of reducing R40, it is more preferable to slow down the stretching speed, and the stretching speed in the second axis is preferably 10,000% / min or less. In addition, the preheating temperature is 20°C or more of the glass transition temperature of the resin and 20°C or less of the glass transition temperature of the resin, and the stretching temperature is preferably 60°C or more of the glass transition temperature of the resin and 20°C or less of the glass transition temperature of the resin.
[0141] In addition, corona treatment can also be applied to at least one side, or an easy-adhesive layer can be applied. As a method for setting a coating layer in an online manner within the film manufacturing process, it is preferred to use a metal wire rod, a gravure roller, etc. to evenly apply a substance obtained by dispersing the coating layer composition in water on a film that has been at least uniaxially stretched, and a method for drying the coating agent while stretching. At this time, as the thickness of the easy-adhesive layer, it is preferably set to more than 10nm and less than 1000nm. In addition, various additives such as antioxidants, heat-resistant stabilizers, ultraviolet absorbers, infrared absorbers, pigments, dyes, organic or inorganic particles, antistatic agents, nucleating agents, etc. can also be added to the easy-adhesive layer. As a resin preferably used for the easy-adhesive layer, from the aspects of adhesion and operability, it is preferably selected from at least one resin of acrylic resin, polyester resin and carbamate resin. In addition, it is also preferred to adopt a method of off-annealing under the conditions of 90 to 200°C.
[0142] Regarding the laminated structure, as described above, two or more extruders may be used for coextrusion to form a laminated polyester film, or a monolayer film may be formed. The laminated structure may be set as required to, for example, an A / B laminated structure obtained by laminating one layer of layer A and layer B, a multilayer laminated structure obtained by alternately laminating multiple layers of layer A and layer B, or a laminated structure obtained by laminating three or more layers. In the case of making a laminated polyester having 101 or more layers, a static mixer or a feed block may be used to merge the layer A composed of the polyester composition of the present invention and the layer B composed of another polyester composition in an alternately laminated manner, so that the two surface layers are layer B.
[0143] Examples of the photoelectric conversion element used in the image display device using the back panel film of the present invention include cameras that obtain information on light from near ultraviolet to visible light and near infrared light with a wavelength of about 300nm to 1500nm, fingerprint authentication sensors, light sensors, distance sensors, etc. As the photoelectric conversion element, a plurality of photoelectric conversion elements can be arranged in one image display device.
[0144] In the image display device of the present invention, light transmitted through the display panel is provided to the photoelectric conversion element arranged at the bottom of the display panel, and the method of transmitting the light through the display can be any method as long as it does not impair the performance of the present invention. For example, the method described in Japanese Patent Application Publication No. 2021-529411 can be cited, but it is not limited thereto.
[0145] Figure 1 FIG. 1 is a schematic diagram for explaining an example of an image display device according to the present invention. Figure 1As shown in FIG. 1 , the image display device 101 includes an array of light-emitting elements for image display, and a frame portion 105 where the array of light-emitting elements is not configured. The array of light-emitting elements for image display includes a screen region 102 where a photographing element 104 for photographing the screen side is configured on the back side of the array of light-emitting elements, and a screen region 103 where no photographing element is configured on the back side. In the portion corresponding to the screen region 102 where the photographing element 104 is configured on the back side of the image display surface, the array of light-emitting elements for image display includes light-emitting elements for image display with high transparency, wherein transparent materials are used for the cathode, the anode, and the light-emitting element substrate, respectively, and in the portion corresponding to the screen region 103 other than this, the array of light-emitting elements for image display may include light-emitting elements for image display with low transparency or light-emitting elements for image display with high transparency.
[0146] The screen area 102 has high transparency, so the image sensor 104 can collect information outside the screen that is incident through the screen area 102. In addition, such an image display device can realize full-screen display. In this example, an example in which the image sensor 104 is configured is described, but other photoelectric conversion elements such as a camera with a different field of view angle from the image sensor 104, a fingerprint authentication sensor, a light sensor, and a distance sensor can also be configured in the area corresponding to the screen area 102.
[0147] The inventors of the present application have conducted in-depth research and found that in an image display device in which a photoelectric conversion element is arranged on the side opposite to the viewer side of the above-mentioned image display light-emitting element array, if the R40 of the film used as the back panel is within the range of 0 nm or more and 1000 nm or less, color unevenness can be significantly suppressed and sensor accuracy can be improved. It is believed that the mechanism by which the generation of color unevenness can be suppressed in the above manner is as follows.
[0148] The image display device of the present invention is an image display device equipped with at least a polarizing plate, an array of light-emitting elements for image display, a back panel of the array of light-emitting elements for image display, and a photoelectric conversion element in the order from the viewer side (the side displaying the image) to the direction in which the array of light-emitting elements for image display exists. If a film having birefringence is clamped by using two optical elements (such as polarizers, etc., hereinafter referred to as "polarizing optical elements") whose transmittances of polarized light are different according to the direction in the plane, it is well known that color unevenness can be observed. On the other hand, in the structure shown this time in which the polarizing plate, the array of light-emitting elements for image display, the back panel, and the photoelectric conversion element are arranged in the order of polarizing plate, the polarizing optical element is no longer included except the polarizing plate, so it is believed that the color unevenness as described above is not observed. However, when light from the outside that is incident obliquely or circularly polarized light emitted from the circular polarizer is incident on the back panel, the transmittance of polarized light (P wave) whose vibration direction of light is parallel to the incident plane and the transmittance of polarized light (S wave) whose vibration direction of light is perpendicular to the incident plane may be different. That is, when light is incident on the surface of the back panel from an oblique direction, the back panel may function as a simulated polarizing optical element. As a result, for the light incident from an oblique direction, that is, the portion corresponding to the end of the photo taken by the camera, it is considered that the optical path for photographing the portion is in a state of being simulated by two polarizing optical elements. It is considered that this has become one of the main reasons for the color unevenness of the camera and the reduction of sensor accuracy. It is considered that since the film used as the back panel is within the above-mentioned phase difference range, it is possible to improve the suppression of color unevenness and sensor accuracy. According to the above mechanism, even when the front phase difference Re is controlled at a low level, when R40 is not included in the range specified in the present invention, it is difficult to suppress color unevenness. In addition, color unevenness can also be suppressed by reducing the difference in transmittance between S waves and P waves. The difference ΔT40 between the average transmittance of P waves when p-polarized light is incident at an angle of 40° and the average transmittance of S waves when s-polarized light is incident at an angle of 40° is preferably 10% or less, and more preferably 7% or less. It is further preferably 5% or less. It should be noted that the wavelength range for calculating ΔT40 is 400 to 800 nm. There is no limitation on the method for making ΔT40 within this range. For example, the following method for controlling the surface structure is preferably adopted: anti-reflection processing is performed on the surface of the film, and a low refractive index layer having a refractive index lower than that of the substrate is made on the surface layer, thereby suppressing the reflectivity at the film interface and improving the transmittance; forming fine protrusions less than 1 / 10 of the wavelength of light on the surface of the film, suppressing the reflectivity at the film interface, thereby improving the transmittance and reducing ΔT40; and so on. The so-called anti-reflection processing here refers to further laminating layers with different refractive indices on the film obtained by film formation by offline coating, vacuum evaporation, etc. For example, it is preferable to adopt a method of evaporating magnesium fluoride on the surface.In the case of forming a low refractive index layer on the surface of the film, when the average value of the refractive index in the length direction and the width direction of the outermost layer of the film (for convenience, referred to as "bare film") before the low refractive index layer is set to n, and the refractive index of the low refractive index layer formed on the surface of the bare film is set to n', from the viewpoint of controlling ΔT40 within the above range, n / n' is preferably 1.08 or more. In addition, from the viewpoint of improving transmittance, the refractive index of the low refractive index layer is preferably 1.35 to 1.58, and more preferably 1.35 to 1.45. From the viewpoint of not imparting performance other than optical performance, the thickness of the low refractive index layer is preferably 1nm to 1μm, and in particular, from the viewpoint of improving transmittance by interfering with visible light, the thickness of the low refractive index layer is preferably 30nm or more and 500nm or less, and more preferably 60nm or more and 200nm or less. In the case of a refractive index of 1.50, the thickness is preferably 60nm or more and 150nm or less, and most preferably 85nm or more and 95nm or less. As a low refractive index layer, for example, by using an acrylic resin as an easy-to-adhesive resin layer, the above refractive index range can be achieved. In addition, by using silica particles with voids inside (hereinafter, sometimes also described as hollow silica particles.) As particles added as a lubricant in the low refractive index layer, the refractive index can also be controlled at a low level, so it is preferably used. The preferred range of the average particle size of the particles added as a lubricant is 40nm or more and 100nm or less, more preferably 40nm or more and 60nm or less. If the average particle size is less than 40nm, the reduction in refractive index is insufficient, and if the average particle size is greater than 100nm, sometimes the film becomes white or the surface concave and convex becomes larger. However, in order to control ΔT40 to such a low area of less than 2%, it is necessary to form a moth-eye structure by embossing or stacking a multilayer vapor deposition layer as an anti-reflection film, etc. to precisely control the surface structure, so the productivity is poor. From this point of view, ΔT40 is preferably more than 2%.
[0149] As for the photoelectric conversion element used in the present invention, the maximum angle that can be collected and identified among the external light irradiated to the image display device, that is, the diagonal viewing angle, is preferably 60 to 140°, and as the lower limit, it is more preferably 70° or more, and more preferably 75° or more. If the diagonal viewing angle becomes too high, the productivity may be reduced. Therefore, as the upper limit, it is preferably 140° or less, more preferably 130° or less, and more preferably 120° or less. According to the above-mentioned mechanism for suppressing the generation of color unevenness, the photoelectric conversion element with a large diagonal viewing angle can be used in the image display device, and a wider range of image information can be accurately collected and identified. In addition, when using a camera as a photoelectric conversion element, from the perspective of taking a clear image, the number of pixels is preferably 7 million pixels or more, and more preferably 12 million pixels or more. There is no limit to the upper limit, but from the perspective of productivity, the upper limit is preferably set to 48 million pixels or less.
[0150] (Measurement of characteristics and evaluation method of effects)
[0151] The method for measuring the characteristics and the method for evaluating the effects in the present invention are as follows.
[0152] (1) Composition of polyester
[0153] The film is hydrolyzed by alkali, and each component is analyzed by gas chromatography or high performance liquid chromatography, and the composition ratio is obtained from the peak area of each component. The dicarboxylic acid constituents and other constituents are measured by high performance liquid chromatography. The measurement conditions can be analyzed by known methods, and an example of the measurement conditions is shown below. It should be noted that during the measurement, the inorganic particles are filtered and separated before implementation.
[0154] Device: Shimadzu LC-10A
[0155] Column: YMC-Pack ODS-A 150×4.6mm S-5μm 120A
[0156] Column temperature: 40°C
[0157] Flow rate: 1.2ml / min
[0158] Detector: UV 240nm
[0159] The diol constituent component and other constituent components can be quantitatively analyzed by a known method using gas chromatography. An example of the measurement conditions is shown below.
[0160] Device: Shimadzu 9A (manufactured by Shimadzu Corporation)
[0161] Column: SUPELCOWAX-10 capillary column 30m
[0162] Column temperature: 140℃~250℃ (heating rate 5℃ / min)
[0163] Flow rate: Nitrogen 25ml / min
[0164] Detector: FID.
[0165] (2) Intrinsic viscosity (IV)
[0166] The sample to be measured (polyester resin (raw material) or polyester film) is dissolved in 100 ml of o-chlorophenol (solution concentration C (sample mass to be measured / solution volume) = 1.2 g / 100 ml), and the viscosity of the solution at 25° C. is measured using an Ostwald viscometer. The viscosity of the solvent is measured in the same manner. Using the obtained solution viscosity and solvent viscosity, [η] is calculated using the following formula (3), and the obtained value is taken as the intrinsic viscosity (IV) (unit: dl / g).
[0167] ηsp / C=[η]+K[η] 2 ·Formula C (3)
[0168] (Here, ηsp=(solution viscosity / solvent viscosity)-1, and K is the Huggins constant (0.343).).
[0169] (3) Film thickness
[0170] The film thickness was measured at five random locations on the film using a micrometer (Standard micrometer 2109S-10 manufactured by MITTOYO Co., Ltd.) in accordance with JIS K7130 (1992) A-2 method. The average value was taken as the film thickness.
[0171] (4) Front phase difference Re, R40, slow axis direction and fast axis direction of the film
[0172] The measurement was performed using a phase difference measuring device ("KOBRA" (registered trademark)-WPR) manufactured by Oji Instruments Co., Ltd. The sample was cut into 3.5 cm × 3.5 cm pieces from the center of the film in the width direction, and the front phase difference Re [nm] and the film orientation angle at a wavelength of 590 nm were measured under the following conditions. The obtained orientation angle direction was taken as the slow axis direction, and the direction orthogonal to the slow axis direction was taken as the fast axis direction. When the length direction and the width direction are unknown, the length direction is consistent with the slow axis direction, and the width direction is consistent with the fast axis direction.
[0173] Measurement method: High phase difference mode
[0174] Dispersion curve parameters: a = 474.44777, b = 2.04281 × 10 7 , c = 250
[0175] λ=750nm, the range of times: 1~5
[0176] In addition, regarding the steps of R40 determination, use Figure 2 The phase difference value is obtained by making a light 205 with a wavelength of 590 nm incident along a surface of a film sample 201 including a fast axis 202 of the film and a vertical axis 203 relative to the film surface at an angle of 40° with the vertical axis as a reference of 0°, and the phase difference value is defined as R40. This measurement is also performed using the same measurement method, dispersion curve parameters, and frequency range as described above.
[0177] For the measurement, five samples were cut out from the center portion in the film width direction, and the measurement was performed on each sample, and the average value was used.
[0178] (5) Young's modulus and elongation at break
[0179] From the center of the film width direction, a strip sample with a length of 150 mm and a width of 10 mm was cut out along the film length direction and the width direction for use. Young's modulus and elongation at break were measured using a tensile testing machine according to the method specified in JIS K7127 (1999). The measurement was carried out under the following conditions, the number of samples was 10, and the measurement was carried out for each sample to obtain the average value.
[0180] Measuring device: Olientech Co., Ltd. film strength and elongation automatic measuring device "Tensilon" (registered trademark) AMF / RTA-100
[0181] Sample size: width 10mm × span 50mm
[0182] Stretching speed: 300mm / min
[0183] Measurement environment: temperature 23°C, humidity 65% RH.
[0184] (6) Bending rigidity
[0185] Regarding the procedure for measuring flexural rigidity, use Figure 3 Provide explanation.
[0186] A rectangular sample 201 having a length of 5 mm in the width direction and 100 mm in the length direction of the measured film is prepared from the central part in the width direction of the film. In a Lupperstei tester (a registered trademark of Toyo Seiki), the sample 201 is set on a chuck 301 in such a way that it becomes a ring with a circumference of 50 mm when formed into a ring. The chucks 301 are brought into contact with each other, and the sample 201 is formed into a ring. A measuring probe is lowered from above the ring at a displacement speed of about 3.5 mm / second, and the load at the time point when the displacement 302 from contact with the ring becomes 10 mm is measured. The obtained value is used as the bending rigidity (mN) of the film in the length direction. In addition, a rectangular sample having a length of 5 mm corresponding to the length direction of the measured film and a length of 100 mm corresponding to the width direction was prepared in the same manner, and the measurement was performed in the same manner, and the obtained value was taken as the bending rigidity (mN) in the width direction of the film. The bending rigidity in the length direction of the film and the bending rigidity in the width direction of the film were measured 5 times each, and the average value of all the values was taken as the bending rigidity (mN).
[0187] (7) Refractive index
[0188] A 3.5 cm × 3.5 cm piece was cut out from the center of the film in the width direction to prepare a measurement sample. Using sodium D line (wavelength 589 nm) as the light source and diiodomethane as the embedding solution, an Abbe refractometer 4T (manufactured by Atago Co., Ltd.) was used at 25°C to measure the refractive index of the film in the length direction, width direction and thickness direction in accordance with JIS K7142 (2014) A method. The refractive index of the film in the length direction was obtained as nx, the refractive index in the width direction was obtained as ny, and the refractive index in the thickness direction was obtained as nz. The refractive index of the test piece placed on the film during the measurement was 1.74. In the case of evaluating a laminated film, each layer was peeled off and measured. The measurement was carried out 5 times, and the average value was used.
[0189] (8) ΔHaze
[0190] The haze measurement device (NDH5000 manufactured by Nippon Denshoku Industries) was used for the measurement. For the sample, a square with a length of 50 mm and a width of 50 mm was cut out from the center of the film in the width direction. The haze measurement was measured in accordance with the method specified in JIS K7136 (2000). For the cut sample, the haze value was calculated under the following conditions, as (haze 1) and (haze 2), respectively. Their values were substituted into formula (4) to calculate Δ haze. The measurement was carried out 5 times, and the average value was used.
[0191] (Haze 1): The haze value when the cut sample is measured directly.
[0192] (Haze 2): The haze value of a sample when the cut sample is left to stand in a Gel aging incubator (GPHH-202 manufactured by Espec Corporation) at 120° C. for 5 hours.
[0193] ΔHaze=(Haze 2)-(Haze 1) Formula (4).
[0194] (9) FT-IR measurement
[0195] A 3.5 cm × 3.5 cm film was cut from the center of the film in the width direction to prepare a measurement sample. A Frontier FT-IR manufactured by Parkin Elmer Co., Ltd. was used, a UATR IR unit was used, the medium crystal was diamond / ZnSe (refractive index 2.4, φ1.5 mm), the light source was MIR, and the measurement range was 4000 to 650 cm -1 The detector was MIR TGS, and the spectral intensity was measured by attenuated total reflection method (ATR method, 1st reflection). The resolution of the spectrometer was set to 4 cm -1 The spectrum was measured by accumulating 16 times. The spectrum was ATR-corrected, and the intensity was the absorbance (arb.unit) at each wavelength. The measurement was performed 5 times, and the average value was used.
[0196] (10) Thermal crystallization heat ΔHc, melting point Tm, crystal melting enthalpy ΔHm, crystallinity Xc of the film
[0197] From the center of the film width direction, 5 mg of sample was measured using an electronic balance and placed in an aluminum sample pan. The Thermo plus ECO2 series DSC vesta manufactured by Rigaku Co., Ltd. was used. According to JIS K7121 (1987) and JIS K7122 (1987), the temperature was raised from 25°C to 300°C at 20°C / min. The data analysis used the Thermo plus ECO2 system manufactured by the company. The heat of thermal crystallization ΔHc, melting point Tm, and crystal melting enthalpy ΔHm were obtained from the obtained DSC data. It should be noted that when multiple melting point peaks are observed, they are named Tm1, Tm2, etc. from the side with the lower peak temperature.
[0198] The crystallinity of the film was calculated by the formula (5): ΔHm0=140.1 J / g.
[0199] Crystallinity Xc (%) = (ΔHm-ΔHc) / ΔHm0×100 Formula (5).
[0200] (11) ΔCp, ΔHg, rigid amorphous content Xra of the film
[0201] The specific heat difference ΔCp (unit: J / (g°C)) and the heat absorption ΔHg (unit: J / g) of the film were measured under the following conditions.
[0202] ·Measurement method: Temperature modulation DSC method
[0203] ·Measurement device: Q1000 manufactured by TA Instruments
[0204] Data processing: TA Instruments "Universal Analysis 2000"
[0205] Atmosphere: Nitrogen flow (50 mL / min)
[0206] Temperature and heat correction: high purity indium (Tm = 156.61 ° C, ΔHm = 28.70 g / J)
[0207] Specific heat correction: Sapphire
[0208] Temperature range: 0~150℃
[0209] Heating rate: 2℃ / min
[0210] Sample volume: 5mg
[0211] Sample container: Aluminum standard container
[0212] The rigid amorphous amount Xra of the film was calculated using the formula (6): ΔCp0=0.4052 J / g°C.
[0213] Rigid amorphous amount Xra (%) = 100 - (Xc + ΔCp / ΔCp0 × 100) formula (6).
[0214] These measurements were performed 5 times, and the average value was used.
[0215] (12) The difference in average transmittance between S-wave and P-wave when incident at an angle of 40° ΔT40
[0216] The following measurement was performed 5 times, and the average value was used.
[0217] (b1) A sample was prepared by cutting out a 3.5 cm × 3.5 cm film from the center of the film in the width direction. A U-4100 spectrophotometer angle variable transmission attachment, a light source cover of 8 mm (H) × 5 mm (W), and a polarizer made by Gramtera were installed, and polarized light as p-polarized light was incident on the film surface as the test specimen at an incident angle of 40°, and the transmission spectrum in the range of wavelengths of 400 to 800 nm was measured. At this time, the measurement was performed in a manner that the slow axis direction of the film was perpendicular to the s-polarized light direction. As the measurement conditions, the slit was set to 2 nm, the gain was set to 2, the scanning speed was set to 600 nm / min, the sampling pitch was set to 1 nm, and a polarizer (manufactured by Kenis Co., Ltd., polarizing film thin type S size, transmittance 0.43, polarization 0.9999, product code 1-115-0820) was installed just in front of the detector, so that only the p-polarized light component in the transmitted light was incident on the detector. From the obtained transmission spectrum, the average value of the transmittance in the wavelength range of 400 to 800 nm was calculated as the p-polarized light component amount Tpp [%] in the transmitted light.
[0218] (b2) The same experiment as (b1) is carried out except that the incident light is changed to s-polarized light relative to the plane of incidence and only s-polarized light is incident on the detector using a polarizer just in front of the detector, and the amount of s-polarized light component Tps [%] in the transmitted light is calculated.
[0219] (b3) Calculate ΔT40 [%] using the following formula (7).
[0220] ΔT40[%]=|Tps-Tpp|, formula (7).
[0221] (13) Density
[0222] A 5 mm square was cut from the center of the film in the width direction, and the density (g / cc) was measured using a density gradient tube using a sodium bromide aqueous solution in accordance with JIS K7112-2 (2023). The measurement was performed three times, and the average value was used.
[0223] (14) Relaxation time of the mobile amorphous phase in TD-NMR measurement after heat treatment at 120°C for 3 minutes
[0224] The relaxation time of the movable amorphous phase was determined using the following apparatus and conditions. The measurement was performed 5 times, and the average value was used.
[0225] Device: Bruker Biospin mq20
[0226] Temperature: 120℃
[0227] Determined core frequency: 19.95MHz
[0228] 90° pulse width: 2.2μsec
[0229] Pulse repetition time: 2sec
[0230] Pulse mode: Solido Echo method
[0231] In the measurement, the film was cut and the film cut to a height of 1 cm was placed in a glass tube with an outer diameter of 10 mm. The film was measured under the above conditions. 1 The decay curve of the spin-spin relaxation response of the H nucleus. The measurement was started after the film was placed in the device and kept at 120°C as the set temperature for 3 minutes. The decay curve obtained was fitted using the least squares method, Gaussian function and exponential function, and separated into three different components. The lifetime of each component is recorded as T1, T2, and T3 from the shorter one. T1 is equivalent to the lifetime of the crystalline component, T2 is equivalent to the lifetime of the rigid amorphous component, and T3 is equivalent to the lifetime of the movable amorphous component.
[0232] (15) Camera visibility (color unevenness evaluation)
[0233] As a simulation evaluation device of the configuration of the present invention, a schematic diagram of a visibility test in a model device configuration of an image display device in which a photoelectric conversion element is arranged below an image display surface is shown in FIG. Figure 4 middle.
[0234] The film 201 cut into 50 mm × 50 mm was overlapped with the polarizing plate 401 (manufactured by Kenis Co., Ltd., thin polarizing film S size, transmittance 0.43, polarization 0.9999, product code 1-115-0820) to prepare a measurement sample. The sample was supported in such a way that the polarizing plate 401 side was at the bottom, and was horizontally set on the surface light source 405 (manufactured by Tritech Co., Ltd., Tribe A4-100). The device 402 with a built-in camera (Samsung "Galaxy" (registered trademark) S10) was used. The device 402 with a built-in camera was set in such a way that the optical axis of the camera lens was perpendicular to the film 201, and the camera was photographed. At this time, the shooting angle 404 was taken in such a way that the entire light emitting range of the surface light source 405 was included. The above operation was performed, and the image captured in the state where the polarizing plate, the back plate, and the camera (photoelectric conversion element) were arranged in this order was observed, and the visibility was judged as described below. It should be noted that in terms of visibility, A, B, and C are considered to be acceptable levels that can be fully used in image display devices.
[0235] A: Almost no interference color is observed as a whole.
[0236] B: Some interference colors can be observed at the corners of the viewing angle, but this is not a problem in practical use.
[0237] C: Interference color is observed as a whole, but it is practically usable.
[0238] D: Interference color is clearly observed, and therefore not suitable for practical use.
[0239] (16) Support
[0240] As samples with a length of 100 mm and a width of 20 mm, two types of samples were prepared: a sample with the long side in the slow axis direction and a sample with the long side in the fast axis direction. For each sample, the sample was placed on a table horizontal to the ground surface in a manner that a 50 mm length portion of the sample protruded. The protruding portion of the sample hangs down, so its relaxation amount is measured. The relaxation amount is defined by the length perpendicular to the ground surface from the upper surface of the portion of the sample placed on the table to the hanging front end of the sample. This measurement was repeated 5 times, and the average value of the bending rigidity in the slow axis direction and the fast axis direction for a total of 10 values was calculated. The support was evaluated according to the following criteria. It should be noted that in terms of support, A and B were judged to be qualified levels that can be fully used in image display devices.
[0241] A: The slack is less than 10 mm, indicating good support.
[0242] B: The amount of slack is 10 mm or more and less than 20 mm, and the support is at a level that is not a problem for practical use.
[0243] C: The amount of slack is 20 mm or more, and the support is insufficient.
[0244] (17) Film Stability
[0245] A film of 300 mm wide and 200 m long (6-inch, 350 mm long core roll) was prepared and rewound on a 3-inch, 350 mm long core under the following conditions, and the following criteria were used to evaluate the film while changing the conveying speed and tension. It should be noted that A and B were judged as levels that can be fully operated during processing.
[0246] A: No tear or damage occurred even when the film was rewound at a speed of 15 m / min and a conveying tension of 70 N / m.
[0247] B: Even when the film was rewound at a speed of 10 m / min and a feeding tension of 70 N / m, no tearing or chipping occurred. However, when the speed was set to 15 m / min, tearing and chipping occurred frequently.
[0248] C: When the film was rewound at a speed of 10 m / min and a conveying tension of 70 N / m, it was torn and chipped.
[0249] (18) Bending resistance
[0250] The measurement was performed using a U-shaped expansion and contraction tester (DLDMLH-FS manufactured by Yuas System Instruments). Figure 5 When explaining, the film sample 201 cut out with a length of 60mm×width 25mm is fixed to an inclined fixture in which the fixture surface is horizontal in a manner that the direction parallel to the long side becomes the bending direction 501, and the central part 502 of the film is bent with a distance between the surfaces of 3mm, and then left to stand for 24 hours. After 24 hours, the bending state is released, taken out of the device, and left to stand with the bent outer side facing downward, and the angle 503 formed by the film sample is measured. The measurement is repeated 5 times for the film sample cut out with the length direction of the film as the long side and the film sample cut out with the width direction as the long side, and the arithmetic mean is calculated as the recovery angle. The fully folded state is recorded as 0°, and the state restored to the original folded state before the film is folded is recorded as 180°, and the angle 403 is read. Using the measurement results with a smaller recovery angle in the length direction and the width direction, the bending resistance is evaluated according to the following benchmarks. It should be noted that bending resistance A and B are levels that can be appropriately used as foldable displays.
[0251] A: The recovery angle is 160° or more, and wrinkles and lifting do not occur when mounted on a foldable display.
[0252] B: The restoration angle is 140° or more and less than 160°, and there is no problem in practical use as a foldable display.
[0253] C: The restoration angle is less than 140°. It can be used practically as an image display device, but is not suitable for practical use as a foldable display.
[0254] (19) Number of times bending reaches fracture
[0255] The film sample was cut into a rectangle of 110 mm (test direction) × 15 mm in width, and a bending test was performed using an MIT bending tester (testing machine No. 702 manufactured by MIT) in accordance with JIS P8115 (2001) under the conditions of a load of 1,000 g, a bending angle of 135° (R: +135°, L: -135°), a bending speed of 175 times / min, and a chuck front end R: 0.38 mm. The number of bends when the film sample broke was taken as the number of times the bending reached the break. The samples collected with the MD direction as the test direction and the samples collected with the TD direction as the test direction were tested three times each, and the arithmetic mean was calculated. It should be noted that in the following evaluation, the evaluation was performed using the larger number of times the bending reached the break in the MD direction or the TD direction, and the repeated bending resistance A and B were at a level that can be appropriately used as a foldable display.
[0256] A: The number of times of bending until breaking is 2000 or more, showing very good repeated bending resistance.
[0257] B: The number of bending times until breaking is 1000 or more and less than 2000 times, and there is no problem in practical use as a foldable display.
[0258] C: The number of times of bending until breaking is less than 1000 times. It can be used practically as an image display device, but is not suitable for practical use as a foldable display.
[0259] Example
[0260] (Manufacture of polyester)
[0261] The polyester resin for film formation is prepared as follows. It should be noted that the expression of mol% is an expression in which the total amount of each component in each of the dicarboxylic acid component and the diol component is set to 100 mol%. In addition, the total amount of the dicarboxylic acid component is equal to the total amount of the diol component in terms of molar ratio.
[0262] (Polyester A)
[0263] A copolymerized polyester resin (intrinsic viscosity: 0.80) containing 92 mol% of a terephthalic acid component as a dicarboxylic acid component, 8 mol% of an isophthalic acid component, 80 mol% of an ethylene glycol component as a diol component, 10 mol% of a 1,4-cyclohexanedimethanol component, and 10 mol% of an isosorbide component.
[0264] (Polyester B)
[0265] A copolyester resin (intrinsic viscosity: 0.80) containing 100 mol% of a terephthalic acid component as a dicarboxylic acid component, 80 mol% of an ethylene glycol component as a diol component, 10 mol% of a 1,4-cyclohexanedimethanol component, and 10 mol% of an isosorbide component.
[0266] (Polyester C)
[0267] A copolyester resin (intrinsic viscosity: 0.80) containing 88 mol% of a terephthalic acid component as a dicarboxylic acid component, 12 mol% of an isophthalic acid component, 80 mol% of an ethylene glycol component as a diol component, 10 mol% of a 1,4-cyclohexanedimethanol component, and 10 mol% of an isosorbide component.
[0268] (Polyester D)
[0269] A copolymerized polyester resin (intrinsic viscosity: 0.80) containing 92 mol% of a terephthalic acid component as a dicarboxylic acid component, 8 mol% of an isophthalic acid component, 73 mol% of an ethylene glycol component as a diol component, 16 mol% of a 1,4-cyclohexanedimethanol component, and 11 mol% of an isosorbide component.
[0270] (Polyester E)
[0271] A copolyester resin (intrinsic viscosity: 0.80) containing 100 mol% of a terephthalic acid component as a dicarboxylic acid component, 73 mol% of an ethylene glycol component as a diol component, 16 mol% of a 1,4-cyclohexanedimethanol component, and 11 mol% of an isosorbide component.
[0272] (Polyester F)
[0273] A copolyester resin (intrinsic viscosity: 0.80) containing 88 mol% of a terephthalic acid component as a dicarboxylic acid component, 12 mol% of an isophthalic acid component, and 100 mol% of an ethylene glycol component as a diol component.
[0274] (Polyester G)
[0275] A polyester resin (intrinsic viscosity: 0.80) containing 100 mol% of a terephthalic acid component as a dicarboxylic acid component and 100 mol% of an ethylene glycol component as a diol component.
[0276] (Polyester H)
[0277] A copolyester resin (intrinsic viscosity: 0.80) containing 95 mol% of a terephthalic acid component as a dicarboxylic acid component, 5 mol% of an isophthalic acid component, and 100 mol% of an ethylene glycol component as a diol component.
[0278] (Polyester I)
[0279] A copolymerized polyester resin (intrinsic viscosity: 0.77) containing 92 mol% of a terephthalic acid component as a dicarboxylic acid component, 8 mol% of an isophthalic acid component, 80 mol% of an ethylene glycol component as a diol component, 10 mol% of a 1,4-cyclohexanedimethanol component, and 10 mol% of an isosorbide component.
[0280] (Polyester J)
[0281] A copolyester resin (intrinsic viscosity: 0.77) containing 100 mol% of a terephthalic acid component as a dicarboxylic acid component, 80 mol% of an ethylene glycol component as a diol component, 10 mol% of a 1,4-cyclohexanedimethanol component, and 10 mol% of an isosorbide component.
[0282] (Polyester K)
[0283] A copolymerized polyester resin (intrinsic viscosity: 0.69) containing 92 mol% of a terephthalic acid component as a dicarboxylic acid component, 8 mol% of an isophthalic acid component, 80 mol% of an ethylene glycol component as a diol component, 10 mol% of a 1,4-cyclohexanedimethanol component, and 10 mol% of an isosorbide component.
[0284] (Polyester L)
[0285] A copolyester resin (intrinsic viscosity: 0.69) containing 100 mol% of a terephthalic acid component as a dicarboxylic acid component, 80 mol% of an ethylene glycol component as a diol component, 10 mol% of a 1,4-cyclohexanedimethanol component, and 10 mol% of an isosorbide component.
[0286] (Polyester M)
[0287] A copolyester resin (intrinsic viscosity: 0.80) containing 92 mol% of a terephthalic acid component as a dicarboxylic acid component, 8 mol% of an isophthalic acid component, 90 mol% of an ethylene glycol component as a diol component, and 10 mol% of an isosorbide component.
[0288] (Polyester N)
[0289] A copolyester resin (intrinsic viscosity: 0.80) containing 100 mol% of a terephthalic acid component as a dicarboxylic acid component, 90 mol% of an ethylene glycol component as a diol component, and 10 mol% of an isosorbide component.
[0290] (Polyester O)
[0291] A copolymerized polyester resin (intrinsic viscosity: 0.80) containing 82 mol% of terephthalic acid as dicarboxylic acid components, 8 mol% of isophthalic acid components, 10 mol% of 2,6-naphthalenedicarboxylic acid components, 90 mol% of ethylene glycol as diol components, and 10 mol% of 1,4-cyclohexanedimethanol components.
[0292] (Polyester P)
[0293] A copolymerized polyester resin (intrinsic viscosity: 0.80) containing 90 mol% of terephthalic acid as a dicarboxylic acid component, 10 mol% of 2,6-naphthalene dicarboxylic acid as a diol component, 90 mol% of ethylene glycol as a diol component, and 10 mol% of 1,4-cyclohexanedimethanol as a diol component.
[0294] (Polyester / PEI resin A)
[0295] The polyester F obtained by the above method and pellets of polyetherimide (PEI) "Ultem" (registered trademark) XH6050-1000 manufactured by SABIC Inobi Precision Co., Ltd. were supplied to a vented twin-screw kneading extruder (manufactured by Nippon Steel Works, Ltd., screw diameter 30 mm, screw length / screw diameter = 45.5) having three kneading paddle kneading sections heated to 280° C. in the same direction, and the pellets were kneaded at a shear rate of 100 sec. -1 The polyester / PEI resin A containing 16% by mass of polyetherimide was obtained by melt extrusion with a residence time of 1 minute. (Intrinsic viscosity: 0.80)
[0296] (Polyester / PEI resin B)
[0297] Polyester G and pellets of polyetherimide (PEI) "Ultem" (registered trademark) XH6050-1000 manufactured by SABIC Inobi Precision Co., Ltd. were supplied to a vented twin-screw kneading extruder (manufactured by Nippon Steel Works, Ltd., screw diameter 30 mm, screw length / screw diameter = 45.5) having three kneading paddle kneading sections heated to 280° C. in the same direction, and the mixture was kneaded at a shear rate of 100 sec. -1 The polyester / PEI resin B containing 16% by mass of polyetherimide was obtained by melt extrusion with a residence time of 1 minute. (Intrinsic viscosity: 0.80)
[0298] (Olefin A)
[0299] “ZEONOR” (registered trademark) 1020R (a resin obtained by subjecting a cyclic olefin and / or a derivative thereof to ring-opening metathesis polymerization and then hydrogenating) manufactured by Zeon Corporation of Japan was used.
[0300] (Easy-adhesion coating layer)
[0301] The easy-adhesion coating layer laminated on the surface of the film was prepared as follows.
[0302] <Coating layer A>
[0303] Resin solution (a): an acrylic resin solution obtained by copolymerizing 64% by mass of methyl methacrylate, 30% by mass of ethyl acrylate, 5% by mass of acrylic acid, and 1% by mass of acrylonitrile.
[0304] Crosslinking agent (b): methylol type melamine crosslinking agent.
[0305] Particles (c): Aqueous dispersion of colloidal silica particles having a particle size of 60 nm.
[0306] Fluorine-based surfactant (d): "Megafluck" (registered trademark) F-444 manufactured by DIC Corporation
[0307] These were mixed at a solid content mass ratio of (a) / (b) / (c) / (d)=30 parts by mass / 8 parts by mass / 2 parts by mass / 0.6 parts by mass. The refractive index after drying was 1.50.
[0308] <Coating layer B>
[0309] Resin solution (e): a solution obtained by mixing 70 parts by mass of a water-soluble coating liquid of a polyester resin composed of an acid component and a diol component, namely terephthalic acid (88 mol%), 5-sodium sulfoisophthalic acid (12 mol%), and ethylene glycol (100 mol%) as an acid component, and 30 parts by mass of an aqueous dispersion of a polyester resin composed of an acid component and a diol component, namely terephthalic acid (50 mol%), isophthalic acid (49 mol%), 5-sodium sulfoisophthalic acid (1 mol%), and ethylene glycol (55 mol%), neopentyl glycol (44 mol%), and polyethylene glycol (molecular weight: 4000) (1 mol%) as a diol component.
[0310] Crosslinking agent (b): hydroxymethyl melamine crosslinking agent
[0311] Crosslinking agent (f): a crosslinking agent containing an oxazoline group
[0312] Particles (g): Aqueous dispersion of colloidal silica particles with a particle size of about 150 nm
[0313] Particles (h): Aqueous dispersion of colloidal silica particles with a particle size of about 300 nm
[0314] Fluorine-based surfactant (d): "Megafluck" (registered trademark) F-444 manufactured by DIC Corporation
[0315] These were mixed at a solid content mass ratio of (e) / (b) / (f) / (g) / (h) / (d)=47 parts by mass / 19 parts by mass / 20 parts by mass / 4.9 parts by mass / 0.7 parts by mass / 0.1 parts by mass. The refractive index after drying was 1.57.
[0316] Hereinafter, the present invention will be described in more detail using examples, but the present invention should not be construed as being limited thereto.
[0317] (Surface processing layer)
[0318] <Offline coating layer>
[0319] 219 parts by mass of 3,3,3-trifluoropropyltrimethoxysilane (KBM-7103 manufactured by Shin-Etsu Silicone Co., Ltd.) was hydrolyzed with 89 parts by mass of 0.5N formic acid while stirring at 20° C.±5° C. After 60 minutes, 412 parts by mass of isopropyl alcohol was added to prepare a treatment liquid (X1).
[0320] Similarly, 158 parts by mass of 3,3,3-trifluoropropyltrimethoxysilane (KBM-7103 manufactured by Shin-Etsu Silicone Co., Ltd.) was hydrolyzed with 41 parts by mass of 1N formic acid while stirring at 30° C.±10° C. After 460 minutes, 521 parts by mass of isopropyl alcohol was added to prepare a treatment liquid (X2).
[0321] Next, a silica slurry (X3) consisting of 144 parts by mass of hollow silica particles ("Slurry" (registered trademark) manufactured by Catalyst Chemicals & Industries, Ltd.) having an average primary particle size of 50 nm and a shell with a porosity of 30% and 560 parts by mass of isopropyl alcohol was prepared.
[0322] After stirring and mixing 720 parts by mass of the treatment liquid (X1), 720 parts by mass of the treatment liquid (X2), 700 parts by mass of the silica slurry (X3), 360 parts by mass of methanol, 4272 parts by mass of isopropyl alcohol, and 713 parts by mass of polypropylene glycol monoethyl ether, 15 parts by mass of acetoacetoxy aluminum as a curing catalyst was added, and the mixture was stirred and mixed again to prepare a coating having a refractive index of 1.45 after drying and curing.
[0323] The prepared coating was applied by a micro gravure coater, dried at 80°C, and then heat treated at 130°C to cure the coating layer, thereby forming an offline coating layer with a thickness of about 0.1 μm. The refractive index of this offline coating layer was 1.45.
[0324] (Example 1)
[0325] Polyester A as the resin component of layer A and polyester B as the resin component of layer B were respectively introduced into two single-screw extruders and melted at 280° C. Then, each was passed through 5 FSS-type leaf disk filters, and while being metered by a gear pump in a discharge ratio of polyester A / polyester B=1 / 4, a three-layer confluence block having a rectangular lamination portion was used to laminate the polyester A layer to the inner layer portion and the polyester B layer to the surface layer portions on both sides, and after being extruded from a T-die in a sheet form, an electrostatic casting method was prepared, and the film was wound on a casting drum at 25° C. to cool and solidify to prepare an unstretched film.
[0326] The unstretched film was stretched to 3.2 times in the length direction at 95°C and then temporarily cooled. Next, the two sides of the uniaxially stretched film were subjected to corona discharge treatment to make the film have a wetting tension of 55 mN / m, and the easy-adhesion coating layer described in Table 1 was applied. Then, it was stretched in stages in the width direction. After being stretched to a total of 3.8 times, it was heat-fixed at a maximum temperature of 228°C in three stages, and then, a 2% relaxation treatment was applied to the length and width directions at 150°C to obtain a film with a thickness of 20 μm. The laminated thickness of the layer obtained from polyester B was 4.0 μm. The thickness of the coating layer after drying was 80 nm. The evaluation results are shown in Tables 2, 3 and 4. The visibility, film-making stability, bending resistance, the number of times the bending reaches fracture, and heat resistance are excellent, but the support is slightly poor due to the thin film thickness.
[0327] (Example 2)
[0328] An unstretched film was prepared by the same method as in Example 1. The unstretched film was stretched to 3.2 times in the length direction at 95°C and then temporarily cooled. Next, the two sides of the uniaxially stretched film were subjected to corona discharge treatment to make the wetting tension of the film 55mN / m, and the easy-adhesion coating layer described in Table 1 was applied. Then, it was stretched in stages in the width direction. After being stretched to a total of 3.8 times, it was heat-fixed in three stages at a maximum temperature of 228°C. Then, a relaxation treatment of 2% was applied to the length and width directions at 150°C to obtain a film with a thickness of 40μm. The laminated thickness of the layer obtained from polyester B was 8.0μm. The thickness of the coating layer after drying was 80nm. The evaluation results are shown in Tables 2, 3 and 4, and are excellent in visibility, film stability, bending resistance, the number of times bending reaches breakage, heat resistance, and support.
[0329] (Example 3)
[0330] The film produced by the same method as in Example 2 was coated to form an off-line coating layer.
[0331] The evaluation results are shown in Tables 2, 3 and 4, showing that the film was excellent in visibility, film forming stability, bending resistance, number of times of bending to breakage, heat resistance and supportability. In addition, the ΔT40 value was also lower than that of Example 2.
[0332] (Examples 4 to 9)
[0333] The composition and film-forming conditions are as shown in Table 1. In addition, the coating thickness is appropriately adjusted, and the same operation as in Example 1 is performed to obtain a film of the thickness described in Table 1. The thickness of the coating layer after drying is 80 nm in Examples 4, 5, 6, 8, and 9, and 92 nm in Example 7. As the film thickness increases, R40 and bending rigidity increase, and there is a tendency for camera visibility and bending resistance to be poor. If a multi-stage stretching process is not adopted, or the relaxation rate in the longitudinal direction is reduced, the amorphous density A becomes smaller, resulting in poor bending. If the refractive index of the easy-to-adhesive formula of the surface layer becomes higher, ΔT40 becomes larger, resulting in poor camera visibility. In addition, when the total thickness of layer B is less than 4.0 μm, the film-forming stability is slightly poor, and sometimes the film breaks during the film-forming process.
[0334] (Examples 10 to 17)
[0335] The composition and film-forming conditions were as shown in Table 1, and the same operation as in Example 1 was performed to obtain a film having a thickness as described in Table 1. In the case where the heat treatment temperature was low compared to the melting point of the resin in the inner layer and nA-nB was 0.02 and low, the camera visibility was poor. On the other hand, in the case where the heat treatment temperature was high compared to the melting point of the resin in the inner layer, the value of Δ haze was slightly poor. In the sample with poor elongation at break, the number of times of bending to break was slightly poor. In the case where isosorbide and cyclohexanedicarboxylic acid were not contained in the surface layer and inner layer of the film, the amorphousness decreased, resulting in slightly poor camera visibility and bending resistance. In the case where they were contained only in the surface layer of the film, the bending resistance was slightly poor, and in the case where they were contained only in the inner layer of the film, the camera visibility was slightly poor.
[0336] (Examples 18 to 21)
[0337] The composition and film-forming conditions were as shown in Table 1, and the same operation as in Example 1 was performed to obtain a film having the thickness described in Table 1. In Example 17, in which the copolymerization amount of the isophthalic acid component of the dicarboxylic acid component of the inner layer was 5 mol%, the melting point of the resin of the inner layer was high and the melting point difference between the resin of the inner layer and the resin of the surface layer was small, so it was difficult to relax the orientation by heat treatment, resulting in slightly poor visibility. In Examples 18, 19, and 20, the IV of the resin was low, and the IV of the film became low, resulting in slightly poor film-forming stability and Δhaze values.
[0338] (Example 22)
[0339] The composition and film forming conditions were as shown in Table 1, and the same operation as in Example 1 was carried out to obtain a film having the thickness described in Table 1. The sample obtained by thinning the film had low bending rigidity and slightly poor supporting properties.
[0340] (Example 23)
[0341] An unstretched film was prepared in the same manner as in Example 1. The unstretched film was stretched in the length direction under the conditions described in Tables 1-2 and then temporarily cooled. Next, the two sides of the uniaxially stretched film were subjected to corona discharge treatment to make the wetting tension of the film 55 mN / m, and the easy-adhesive coating layer described in Table 1 was applied. Then, it was stretched in stages in the width direction. After stretching to a total of 3.8 times, it was heat-fixed in three stages at a maximum temperature of 228°C, and then, at 150°C, a 2% relaxation treatment was applied to the length and width directions to obtain a film with a thickness of 40 μm. The total stacking thickness of the layers obtained from polyester B was 8.0 μm. The thickness of the coating layer after drying was 80 nm. As shown in Tables 2 to 4, the evaluation results were excellent in terms of film stability, the number of times the film was bent to break, heat resistance, and support, but the result of not containing the 1,4-cyclohexanedimethanol component was that visibility and bending resistance were slightly poor.
[0342] (Examples 24 and 25)
[0343] An unstretched film was prepared by the same method as in Example 1. The unstretched film was stretched in the length direction under the conditions described in Table 1-2 and then temporarily cooled. Next, the two sides of the uniaxially stretched film were subjected to corona discharge treatment to make the wetting tension of the film 55mN / m, and the easy-adhesive coating layer described in Table 1-2 was applied, and then, it was stretched in stages in the width direction. After stretching to a total of 3.8 times, it was heat-fixed at a maximum temperature of 228°C in three stages, and then, a 2% relaxation treatment was applied to the length and width directions at 150°C to obtain a film with a thickness of 40μm. The total stacking thickness of the layer obtained from polyester B is 8.0μm. The thickness of the coating layer after drying is 80nm. As shown in Tables 2 to 4, Example 24 containing naphthalene dicarboxylic acid as a copolymer component and Example 25 containing PEI are excellent in visibility, film stability, bending resistance, the number of times bending to break, heat resistance, and support.
[0344] (Example 26)
[0345] The composition and film-forming conditions were as shown in Table 1, and the same operation as in Example 1 was performed to obtain a film having the thickness described in Table 1. It should be noted that since the stretching process was not performed, the coating thickness was reduced compared with Example 1 when the easy-adhesion layer was applied, and the thickness of the coating layer after drying was adjusted to 80 nm. In the film having an olefin resin component, R40 was low, but the elongation at break was low, resulting in a slightly poor number of times of bending to breakage.
[0346] (Comparative Examples 1 and 2)
[0347] The composition and film forming conditions were as shown in Table 1, and the same operation as in Example 1 was carried out to obtain a film having a thickness described in Table 1. R40 was a value exceeding 1000 nm, and the visibility was poor in all cases.
[0348] (Comparative Example 3)
[0349] An unstretched film was prepared by the same method as in Example 1. Both sides of the unstretched film were subjected to corona discharge treatment to make the wetting tension of the film 55 mN / m, and the easy-adhesive coating layer described in Table 1-2 was applied. Then, the film was biaxially stretched to 3.4 times in both the length and width directions, and then thermally fixed at a maximum temperature of 230°C. Then, a 2% relaxation treatment was performed in the length and width directions at 150°C to obtain a film with a thickness of 40 μm. The total stacking thickness of the layers obtained from polyester B was 8.0 μm. Compared with Example 1, the total stretching ratio after coating the easy-adhesive layer was high, so the coating thickness when the easy-adhesive layer was coated was thickened. The thickness of the coating layer after drying was 80 nm. R40 was a value exceeding 1000 nm, and as a result, the visibility was poor.
[0350] [Table 1-1]
[0351] Table 1
[0352]
[0353] [Table 1-2]
[0354]
[0355] [Table 2]
[0356]
[0357] [Table 3]
[0358] Table: 3
[0359]
[0360] [Table 4]
[0361] Table 4
[0362]
[0363] Industrial Availability
[0364] When the back panel film of the present invention is used in an image display device, normal image information can be collected and recognized in a photoelectric conversion element disposed below the image display surface, and the industrial applicability is extremely high. In addition, the back panel film of the present invention can also be suitably used as a screen protection film used in all displays, a polarizer protection film used in a liquid crystal display or an organic EL display, a touch panel substrate film forming a transparent conductive layer, or a film for projecting a hologram.
[0365] Description of Reference Numerals
[0366] 101: Image display device
[0367] 102: The image sensor is arranged in the screen area on the back side of the image display surface
[0368] 103: The image sensor is not arranged in the screen area on the back side of the image display surface
[0369] 104: Photographic element
[0370] 105: Border part
[0371] 201: Film (back panel)
[0372] 202: Fast Axis
[0373] 203: Vertical axis
[0374] 204: Angle of incidence
[0375] 205: Light
[0376] 301: The chuck of ループスティフネステスタ
[0377] 302: Displacement
[0378] 401: Polarizing plate
[0379] 402: Device with built-in camera
[0380] 403: Ultra-wide-angle lens
[0381] 404: Shooting angle
[0382] 405: Area light source
[0383] 501: Bending direction
[0384] 502: Central part of the membrane
[0385] 503: Angle formed by the film sample.
Claims
1. A back panel film, which is a back panel film for an image display device, wherein the image display device is equipped with a polarizing plate, an array of light-emitting elements for image display, a back panel and a photoelectric conversion element in sequence when observed from the viewer's side, and the phase difference value of the back panel film is greater than 0nm and less than 1000nm, and the phase difference value is obtained by making light with a wavelength of 590nm incident at an incident angle of 40° along a plane including a fast axis of the film and a vertical axis relative to the film surface, with the vertical axis as a reference 0°. 2 . The back sheet film according to claim 1 , comprising a biaxially oriented polyester film as one of its components.
3. The back panel film according to claim 2, wherein the biaxially oriented polyester film is a single-layer film or a film formed by stacking a plurality of layers, and comprises at least one polyester resin layer, wherein the polyester resin layer contains 6 mol % or more of isophthalic acid components in the total dicarboxylic acid components of the polyester resin constituting the layer.
4. The back panel film according to claim 2, wherein the polyester constituting the biaxially oriented polyester film is a polyester obtained by polymerization or copolymerization of at least one selected from naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, fluorene derivatives, terephthalic acid, bisphenol A, isosorbide, cyclohexanedimethanol and their ester-forming derivatives, or a polyester containing polyetherimide. 5 . The back sheet film according to claim 2 , wherein the crystallinity is 30% or less and the rigid amorphous content is 20% or more and 50% or less.
6. The back panel film according to claim 1, which is a film formed by laminating two or more layers, and satisfies the following formula (1) when the thickness-direction refractive index of the layer with the largest thickness-direction refractive index is nA and the thickness-direction refractive index of the layer with the smallest thickness-direction refractive index is nB: nA-nB ≥ 0.02 (1). 7 . The back sheet film according to claim 1 , wherein the increase in haze (Δhaze) when heat-treated at 120° C. for 5 hours is 0% to 2.0%. 8 . The back sheet film according to claim 2 , wherein the biaxially oriented polyester film has a relaxation time of a movable amorphous phase of 0.200 ms or less in TD-NMR measurement after heat treatment at 120° C. for 3 minutes.
9. The back sheet film according to claim 2, wherein the biaxially oriented polyester film is composed of a plurality of layers, and in the Fourier transform infrared spectroscopy (FT-IR) spectrum of the thickest layer among the layers constituting the film, the thickness of the film is 0.1777 cm / s. -1 The spectral intensity r2 observed at 1388 cm -1 The ratio R(r2 / r1) of the spectral intensity r1 observed at the position satisfies the following formula (2): 1.0 < R < 1.8 (2)。 10 . The back sheet film according to claim 1 , wherein the flexural rigidity is 0.2 mN or more and 20.0 mN or less in both the longitudinal direction and the width direction.
11. According to the back panel film according to claim 2, the amorphous density A of the biaxially oriented polyester film is greater than 1.0, and the amorphous density A is calculated by ΔHg / ΔCp, wherein the ΔHg / ΔCp is obtained by dividing the endothermic amount ΔHg observed in the irreversible curve of the temperature-modulated DSC (30-150°C) by the specific heat difference ΔCp before and after the glass transition temperature observed in the reversible curve. 12 . The back sheet film according to claim 1 , wherein the restoration angle is 140° or more in both the longitudinal direction and the width direction. 13 . The back sheet film according to claim 1 , wherein the elongation at break is 50% or more in both the longitudinal direction and the width direction. 14 . The back sheet film according to claim 1 , wherein the number of times the film is bent to break as evaluated by an MIT bending tester is 1,000 or more times in both the longitudinal direction and the width direction. 15 . The back plate film according to claim 1 , wherein the difference between the average transmittance of P waves when p-polarized light is incident at an incident angle of 40° and the average transmittance of S waves when s-polarized light is incident at an incident angle of 40° is 10% or less.
16. A polyester film, comprising a dicarboxylic acid component and a diol component, wherein the terephthalic acid component in the dicarboxylic acid component is 50 mol% or more and 95 mol% or less, the ethylene glycol component in the diol component is 50 mol% or more and 95 mol% or less, the melting point observed on the lowest temperature side is 240°C or less, the density is 1.360 g / cc or less, and the phase difference value obtained by causing light of a wavelength of 590 nm to be incident at an incident angle of 40° with the vertical axis as a reference of 0° along a plane including the fast axis of the film and the vertical axis relative to the film surface is 0 nm or more and 1000 nm or less.
17. The polyester film according to claim 16, which is a single-layer film or a film formed by laminating a plurality of layers, and has at least one polyester resin layer, wherein the polyester resin layer contains 6 mol % or more of isophthalic acid components in all dicarboxylic acid components constituting the polyester resin layer.
18. The polyester film according to claim 16, wherein the polyester constituting the polyester film is a polyester obtained by polymerizing or copolymerizing at least one selected from naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, fluorene derivatives, terephthalic acid, bisphenol A, isosorbide, cyclohexanedimethanol and ester-forming derivatives thereof, or a polyester containing polyetherimide. 19 . The polyester film according to claim 16 , wherein the degree of crystallinity is 30% or less and the amount of rigid amorphous is 20% or more and 50% or less. 20 . The polyester film according to claim 16 , wherein the relaxation time of the movable amorphous phase in TD-NMR measurement after heat treatment at 120° C. for 3 minutes is 0.200 ms or less.
21. The polyester film according to claim 16, wherein in the Fourier transform infrared spectroscopy (FT-IR) spectrum of the thickest layer among the layers constituting the film, -1 The spectral intensity r2 observed at 1388 cm -1 The ratio R(r2 / r1) of the spectral intensity r1 observed at the position satisfies the following formula (2): 1.0 < R < 1.8 (2)。 22 . The polyester film according to claim 16 , which has a bending rigidity of 0.2 mN to 20.0 mN both in the longitudinal direction and in the width direction.
23. The polyester film according to claim 16, has an amorphous density A of greater than 1.0, and the amorphous density A is calculated by ΔHg / ΔCp, wherein ΔHg / ΔCp is obtained by dividing the endothermic amount ΔHg observed in the irreversible curve of temperature-modulated DSC (30-150°C) by the specific heat difference ΔCp before and after the glass transition temperature observed in the reversible curve.
24. The polyester film according to claim 16, which has a breaking elongation of 50% or more in both the longitudinal direction and the width direction. 25 . An image display device comprising the back panel film according to claim 1 or the polyester film according to claim 16 . 26 . The image display device according to claim 25 , wherein the light emitting element array for an image display device used in the image display device is an organic electroluminescent element array. 27 . The image display device according to claim 25 , wherein the photoelectric conversion element mounted on the image display device can receive light in an angle range of not less than 60° and not more than 140°. 28 . A foldable display equipped with the back panel film according to claim 1 or the polyester film according to claim 16 . 29 . A device comprising an image display device as one of its components, wherein the image display device is provided with the back plate film according to claim 1 or the polyester film according to claim 16 .