Multi-layer release stack for light-induced transfer of components
By using the release stack structure of the light absorbing layer, decomposition layer, melting layer and adhesive layer during component transfer, and using beam heating and bubble formation technology, efficiency and control problems during component transfer are solved, achieving high efficiency, Low damage to parts transfer.
Patent Information
- Application Number
- CN202280095245.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2022-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to balance between efficiency, yield and control levels during the light-induced transfer of components from the donor substrate to the acceptor substrate, resulting in uncontrolled transfer process, the components are susceptible to thermal damage, and the transfer speed is slow.
Using a release stack composed of a light absorbing layer, a decomposition layer, a melting layer and an adhesive layer, the light absorbing layer is heated by a light beam so that its absorbing heat is transmitted to the melting layer. The decomposition layer and the decomposition layer evaporate to form bubbles, increasing the pressure inside the layer It stimulates component release and reduces shear force and thermal damage through the segmented layer structure to achieve efficient and low shock wave transfer of components.
Fast and controlled transfer of components is achieved, reducing thermal damage, improving efficiency and yield of the transfer process, while reducing the impact on adjacent molds.
Smart Images

Figure CN119072779A_ABST
Abstract
Description
[0001] Technical Field and Background Art
[0002] The present disclosure relates to methods and systems for light-induced transfer of components, such as chips, from a donor substrate to an acceptor substrate. The present disclosure also relates to a donor substrate for use in such a method or system.
[0003] Controlled transfer of small components has various applications, for example in the placement of μLEDs. Light-induced transfer can be used to selectively transfer components from a donor substrate to a receptor substrate. To facilitate the transfer, a release stack can be provided between the donor substrate and the components. In one technique, the components are glued to a carrier substrate and released from the carrier due to rapid blister formation. In another technique, a flat glass sheet with a light absorbing layer is coated with glue. When the light absorbing layer is rapidly heated by a light pulse, the components can be released due to decomposition or melting of the glue.
[0004] For each known method, there is a trade-off between efficiency (i.e., speed), throughput, and level of control. None of these methods provide the desired level of control over the transfer process. Faster techniques provide lower throughput. Further improvements in controlled transfer and placement of components are still needed. Summary of the invention
[0005] Some aspects of the present disclosure relate to methods and systems for light-induced transfer of components from a donor substrate to an acceptor substrate. Other or additional aspects relate to donor substrates for use in such methods or systems. Typically, a transparent carrier is configured to carry the components facing the acceptor substrate, and a release stack is disposed between the transparent carrier and the components for releasing one or more of the components from the donor substrate to the acceptor substrate after the release stack is irradiated by a light beam through the transparent carrier.
[0006] As described herein, the release stack of the donor substrate includes a light absorbing layer, a decomposition layer, a melting layer and an adhesive layer. The light absorbing layer is arranged between the transparent carrier and the decomposition layer. By providing a light absorbing layer with a relatively high absorption coefficient, the light beam can be efficiently absorbed, so that the light absorbing layer is heated. By providing a heated light absorbing layer in thermal contact with the melting layer via the decomposition layer, the absorbed heat can be conducted to the melting layer by the decomposition layer, so that the temperature of the decomposition layer and the melting layer can be increased. By providing a relatively low melting temperature for the material of the melting layer, this material can be easily melted. By providing a relatively high melting temperature (at least higher than the melting temperature of the melting layer) for the light absorbing layer, the light absorbing layer can remain solid when the melting layer is melted by the heat conducted from the light absorbing layer. By providing an adhesive layer between the component and the melting layer, the component can easily adhere to the melting layer when the melting layer is solid. In addition, when the melting layer melts, this adhesion can be released. By providing an evaporation temperature between the melting temperature of the melting layer and the melting temperature of the light absorbing layer for the decomposition layer, the material of the decomposition layer will begin to evaporate after the melting layer melts. In the decomposition layer, the formation of bubbles increases the pressure in the layer, causing the decomposition layer to form a convex shape below the molten molten layer. This stimulates the release of the components by increasing the contact angle with the adhesive layer at the appropriate time. Therefore, in the absence of the decomposition layer, the release of the components will be accelerated. Therefore, due to the acceleration of the release, the total heat transfer to the components is limited, which in turn offsets the potential loss of the components due to thermal damage. In addition, by at least segmenting the adhesive layer between the components, the components can be transferred more easily. For example, if a part of the adhesive layer can be released with the components without being connected to the surrounding parts of the adhesive layer, such as keeping adjacent (untransferred) components or other parts of the adhesive layer, the shear force during the transfer can be alleviated. By segmenting the decomposition layer, bubble formation and the curvature becoming convex are limited to the area below the components (or if necessary, even its smaller sub-area). In addition, the molten layer and / or the light absorbing layer can be segmented to provide further advantages, such as further separating and / or isolating the heat of the corresponding stack. Although segmentation has specific advantages, in principle, the components can also be released without the need for segmentation. For example, when the molten layer between the component and the light absorbing layer is locally melted and the adhesion is reduced, a portion of the (continuous) adhesive layer holding the component may be relatively fragile and simply break from the surrounding adhesive layer. For example, the component can be pulled, pushed or otherwise released from the carrier by various forces (such as gravity and / or by optional gas generation to dewet or accumulate the molten material).
[0007] Typically, the region of the light absorbing layer (e.g., forming a portion of the release stack that holds the corresponding component) is irradiated with a light beam through a transparent carrier. This may cause the corresponding portion of the light absorbing layer to be heated. The heat can then be conducted to the adjacent melting layer of the release stack, thereby preferably at least partially melting the adjacent melting layer when the corresponding portion of the light absorbing layer remains substantially solid. Therefore, at least partial melting of the adjacent melting layer may cause a loss of adhesion between the adjacent melting layer and the corresponding portion of the adhesive layer of the release stack (adhering the corresponding component to the adjacent melting layer). Therefore, the loss of adhesion may cause the release and transfer of the corresponding component. For example, one or more light sources and / or masks are configured and controlled to generate one or more light beams for transferring the corresponding component as described herein.
[0008] In some embodiments, in addition to the decomposition layer providing its function through bubble formation resulting in pressure accumulation in the layer, the low gas generation melting layer and adhesive layer in the laser release stack are used to quickly transfer the components from the carrier toward the receptor substrate. Due to the low pressure accumulation, the components can be transferred at a low speed (minimal or no shock wave), and due to the less turbulent air (gas) around, the components can be substantially prevented from rotating during transfer. It is noted that the bubbles formed in the decomposition layer are confined to the layer in the stack with little or no degassing. In one embodiment, the stack includes a thermally stable light absorbing layer, a melting layer and an adhesive layer, or is substantially composed of a thermally stable light absorbing layer, a melting layer and an adhesive layer. Preferably, the melting layer is a metal layer with a relatively low melting temperature. More preferably, the light absorbing layer is also a metal layer, but has a relatively high melting temperature. More preferably, the decomposition layer is also a metal layer, and its evaporation temperature is between the melting temperatures of the melting layer and the light absorbing layer. The present invention is not limited to metal decomposition layers, and other materials or alloys with suitable properties can be applied. Most preferably, the adhesive layer consists essentially of a polymer adhesive whose decomposition temperature is higher than the melting temperature of the metal molten layer and / or closely matches it. As a further advantageous (but not essential) preference, the decomposition layer has a melting temperature also higher than the melting temperature of the molten layer, so that melting starts first in the molten layer.
[0009] In some embodiments, the laser beam or other light source quickly and fully heats the light absorbing layer so that the lower metal layer begins to melt. In the molten state, the polymer adhesive that binds the component to the metal molten layer may be released, for example, due to the dewetting effect. Since the surface tension of the liquid metal is usually much higher than the surface energy of the solid polymer, the adhesion can be released between the two layers. In contrast, since the surface energy of the solid metal layer is usually very high, the metal molten layer can adhere to the metal decomposition layer as long as its melting temperature is higher than the melting temperature of the molten layer (as described above). Therefore, the metal of the molten molten layer will be beneficial to the metal of the (usually still solid) decomposition layer, and due to dewetting, the adhesive layer will be released. When the temperature of the decomposition layer is raised to above its evaporation temperature, the process is accelerated, and bubbles are formed by the gas generation in the decomposition layer below the molten layer. This will cause the curvature of the decomposition layer surface and the liquid molten layer thereon to increase (become convex), thereby stimulating the early release of the adhesive. For example, only the polymer part is transferred with the component. After the transfer, the polymer layer can be removed from the component, for example, by dry etching or thermal decomposition.
[0010] In some embodiments, in order to increase the transfer speed of the component, the polymer adhesive can be adjusted so that it decomposes slightly at the melting point of the molten layer. During melting, for example, due to the high surface tension of the molten metal, the contact area between the adhesive and the molten layer can be reduced. Therefore, the material may tend to curl. Although the evaporation (decomposition) temperature of polymer materials (such as SU-8) at low heating rates is about 350°C, at very high heating rates, the decomposition of the polymer tends to occur at much higher temperatures. Selecting a polymer / metal combination can release the component without generating any gas, wherein the polymer has a higher decomposition temperature as the melting temperature of the metal (e.g., Sn+SU8, Zn+polyimide). Advantageously, the evaporation temperature of the decomposed layer is selected so that in the process, when the contact area between the molten layer and the adhesive layer is reduced, bubble formation and convex surface formation occur so as to trigger the release at that moment. In addition, for example, gravity or electrostatic force can be used to release the component from the carrier and transfer it toward the receptor substrate. Generally, it is preferred to keep it below the boiling point (evaporation temperature) of the metal molten material. Otherwise, the evaporated metal may cause additional pressure and deposit on the cooler surrounding surface.
[0011] In addition to controlling the amount of gas generated, it is also preferred to heat the light absorbing layer as uniformly as possible to ensure that the metal molten layer melts at the same time. In some embodiments, a flat-top beam profile is used, which specifically heats the stack above one component and does not interfere with any adjacent components. Since it is best to have very narrow cut streets (e.g., ≤5μm) between components to reduce the amount of substrate waste, selective heating of individual components may become increasingly difficult. Especially when increasing the transfer speed, the timing jitter on the laser may be more difficult to control. Therefore, it is preferred to use a mask that is precisely aligned with the component and fine-tune the laser pulse to the correct size.
[0012] Since typically only a small portion of a component needs to be transferred (e.g. for μLED displays), the laser pulse can be (much) larger than the component. For example, a relatively large flat-top beam in combination with a mask can produce a robust process that does not require a precise and expensive laser positioning control system. For example, the maximum laser spot size can be calculated as the component spacing minus the component size minus twice the laser accuracy. For example: 2×200pm (component spacing)-40pm (component size)-10pm (laser accuracy)=350μm. At these large spot sizes, it may be relatively easy to obtain a uniform heat flux in the middle, especially with beam shaping optics such as πShaper.
[0013] To reduce the heat affected zone and further limit the amount of gas generated, in some embodiments, the size of the metal melt layer below the component is reduced. For example, in order to automatically center the metal melt layer under the component, the layer can be under-etched in the etching bath. The more centralized the component release, the better the transfer process.
[0014] Other or further improvements can come from the strategic transfer of the components to ensure that they are pushed directly towards the receptor substrate. For example, in the event that there is any gas generation under the component, generally such gas will be most likely to escape where the flow resistance is lowest. Even if the heat flux is almost completely uniform, uneven pressure around the component may lead to undesirable component trajectory, such as rotation of the component during transfer. To alleviate this problem, for example a checkerboard approach can be used, in which the components are transferred in an alternative manner. By ensuring that the component to be transferred is either surrounded by adjacent components on the opposite side or not, the pressure build-up around the transferred component can be more uniform. When the trajectory of the component can be better controlled in a straight-down direction, a larger transfer gap can be achieved, which may be beneficial for industrialization as height positioning does not need to be very precise.
[0015] To improve performance, for example, the heat flux and the fluence can be controlled. Preferably, the light absorbing layer is heated without reaching its melting or evaporation temperature. In addition, high-intensity light preferably does not reach the component to prevent damage. Regarding the layer thickness of the metal molten layer, the thicker the layer, the higher the flux required to melt the entire layer. In addition, it is possible for the metals of different layers to diffuse and form alloys. If there is relatively too much molten metal, the light absorbing layer may diffuse completely into the molten pool. If the light absorbing layer melts, non-uniform effects may occur. In order to control the melting time, the pulse time and the fluence can be controlled. Preferably, the pulse time is in the order of nanoseconds or picoseconds. Shorter pulses in the order of femtoseconds may result in "cold" ablation of the light absorbing layer, while longer pulses in the order of microseconds may increase the heat affected area. In general, longer pulses may also be less effective because most of the heat may disappear due to heat dissipation of the carrier and the component. The thickness of the adhesive layer can be increased to reduce the heat flow toward the component. By accelerating the release of the component with the help of the decomposition layer, the duration of heat transfer to the component can be reduced to prevent thermal damage to it, while allowing the adhesive layer to be thinner. Although relatively high temperatures are achieved at the light absorbing layer and the melting layer, the component can be kept relatively cool in this way. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] These and other features, aspects, and advantages of the apparatus, systems, and methods of the present disclosure will become better understood through the following description, appended claims, and accompanying drawings, in which:
[0017] Figure 1A Transferring a component from a donor substrate to a receptor substrate by irradiating the release stack is shown;
[0018] Figure 1B shows the relative temperatures and sequence of releasing components by light-induced heating to release selected layers in a stack;
[0019] Figure 2A and Figure 2B Other aspects including cutting and / or etching to release portions of the stack are shown;
[0020] Figure 3A The masking of the light pulses to form a relatively narrow beam and the relative thickness of the layers are shown;
[0021] Figure 3B The sequential release of components is shown;
[0022] Figure 4A and Figure 4B A photograph of the part transferred to the acceptor substrate is shown;
[0023] Figure 4C A portion of the remaining stack on the donor substrate is shown;
[0024] Figure 5A and Figure 5B The other layers in the release stack are shown;
[0025] Figure 6 The sequence of releasing components by multiple light pulses is shown. DETAILED DESCRIPTION
[0026] The terms used to describe specific embodiments are not intended to limit the present invention. As used herein, the singular forms "a", "an" and "the" are also intended to include plural forms unless the context clearly indicates otherwise. The term "and / or" includes any and all combinations of one or more associated listed items. It will be understood that the terms "comprises" and / or "comprising" specify the presence of the stated features, but do not exclude the presence or addition of one or more other features. It will be further understood that the terms "essentially consisting of..." and "essentially consisting of..." used when referring to materials (e.g., metals, semiconductors, polymers) herein mean that other components may be present as long as these components do not have a substantial effect on the basic properties of the compound or composition. Alternatively or additionally, these terms can be used to represent a major component, such as a mass percentage of >90%, >95%, >99, >99.9% or 100% (or simply "consisting of..."). It will be further understood that when a particular step of a method is referred to as a subsequent step of another step, unless otherwise specified, it may directly follow the other step, or one or more intermediate steps may be performed before performing the particular step. Likewise, it will be understood that when connections are described between structures or components, such connections may be made directly or through intermediate structures or components unless otherwise stated.
[0027] The present invention is described more fully below with reference to the accompanying drawings, in which embodiments of the invention are shown. In the accompanying drawings, the absolute and relative sizes of systems, components, layers and regions may be exaggerated for clarity. Embodiments may be described with reference to schematic and / or cross-sectional views of possible idealized embodiments and intermediate structures of the present invention. In the description and drawings, the same reference numerals always represent the same elements. Relative terms and their derivatives should be interpreted as referring to the orientation shown in the drawings being described or discussed at the time. These relative terms are for ease of description and do not require that the system be constructed or operated in a specific orientation unless otherwise specified.
[0028] This document relates to deploying a low gas generation laser release stack so that parts are quickly transferred from a carrier toward a receptor substrate. In the present invention, a self-limiting bubble formation mechanism is applied in the stack configuration, causing a convex curvature, which enables the molten molten layer from the mold to be dehumidified quickly and efficiently during the transfer process. Therefore, first, due to low pressure accumulation, the parts are transferred at a low speed (without shock waves), and in the absence of turbulent ambient air or gas, the parts do not tend to rotate during the transfer. This increases the yield of the final product by improved control of the correctness of the transfer. Secondly, the curvature formed by the self-limiting bubbles in the decomposition layer helps to more efficiently dehumidify the molten molten layer with micro-components during the transfer process. This accelerates the release, and therefore shortens the release time, and thereby shortens the contact time between the hot molten metal layer and the polymer adhesive layer. Thereby achieving a high level of control over the transfer process, while providing high-yield macro components via an efficient transfer process with a large throughput. It further realizes the laser mold transfer of larger components, and also reduces the debris from the mold during the laser mold release process. The stack consists of a thermally stable light absorbing layer, a thin decomposition layer that forms bubbles, a metal melting layer and an adhesive layer. The melting and evaporation temperatures of each layer are carefully selected to provide a specific functional effect at a specific time during the expiration period.
[0029] The laser release stack consists of four functional layers: a light absorbing metal layer with a high melting temperature, a very thin degradation layer that causes bubble formation with an evaporation temperature higher than the temperature of the metal molten layer (e.g., preferably a metal with the desired evaporation temperature, but in some cases a thin oxide such as Al2O3 or SiO2, or a polymer with a high degradation temperature can also be applied), a metal layer with a low melting temperature, and a polymer binder with a decomposition temperature that closely matches the melting temperature of the metal molten layer.
[0030] The working principle is that the laser beam (e.g., with a relatively long pulse of the order of tens of microseconds) quickly and sufficiently heats the light absorbing layer so that the underlying metal layer begins to melt. Note that the decomposition layer deposited between the metal layers is very thin (only tens of nanometers) to prevent the flow of heat from the absorbing layer to the molten layer from being blocked. When the molten layer reaches its melting temperature during the relatively long pulse and changes from solid to liquid, the polymer adhesive that binds the component to the metal molten layer begins to release due to the dewetting effect. This also occurs in the absence of a decomposition layer, because the surface tension of the liquid metal is much higher than the surface energy of the solid polymer, and therefore the adhesion between the two layers is easily lost; in contrast, since the surface energy of the solid metal layer is usually very high, the metal molten layer will adhere to the metal layer, such as the light absorbing layer. Therefore, the molten metal tends to dewet from the polymer part, thereby releasing the component together with the polymer part. However, due to the unfavorable aspect ratio of the molten layer, this process requires a lot of time. The thickness of the molten layer can be in the submicron range, because thick metal layers require a large energy dose to reach and maintain a molten state, and therefore, thermal damage to the component will be caused. The lateral steps of the molten layer can be on the order of tens of microns, matching the dimensions of a typical component. Due to this aspect ratio, the thin melt bridge formed by the molten molten layer requires a lot of time to naturally dewet from the large polymer surface for subsequent mold release. This increases the likelihood of thermal damage to the component, which is undesirable.
[0031] In order to accelerate the dewetting process, so that the laser pulse still pumps energy into the release stack when the molten layer melts, the decomposition layer of the present invention intervenes. Since its evaporation temperature is higher than the melting temperature of the molten layer and lower than the melting temperature of the light absorbing layer, during the above process, the thin degraded layer reaches its evaporation temperature and bubbles are thus formed in the layer, which makes its surface convex. The increased curvature increases the contact angle between the molten layer and the adhesive layer and thus stimulates release. Importantly, the bubbles can be laterally confined by the etching or singulation process, preventing them from propagating laterally and thus preventing them from affecting adjacent molds that are closely spaced on the wafer.
[0032] The present invention makes it possible to selectively transfer parts with small cut lanes in between. This is because the formation of bubbles is not the main driving factor of the transfer process and can therefore occur in a confined area below the parts to be transferred. The small cut lanes will increase the number of parts that can be accommodated on a single wafer. These small cut lanes are not obtainable in blister assisted laser transfer processes, where the formation of bubbles is the main driving factor. This is because in conventional methods, since blistering is the main driving factor, the required blisters need to be large and even larger than the parts. Larger cut lanes are needed to prevent premature release of adjacent parts. In addition to this, conventional blister assisted methods require a focused laser beam and therefore require precise laser alignment to ensure that the parts are transferred vertically downward.
[0033] An important advantage of the present invention is the use of a four-layer stack, which makes it possible to transfer parts with limited or no gas generation (the gas generated by the decomposition layer is very limited, and only microbubbles need to be formed, without actual thrust for the mold). This allows limiting the transfer speed of the parts and ensuring that they follow the desired trajectory. The choice of materials is important. The surface energy, melting temperature and evaporation temperature need to match to achieve the desired transfer effect. The self-constraint of the bubbles formed allows limiting the impact on adjacent molds during laser mold release, while the out-of-plane deformation of the molten molten layer caused by the formation of microbubbles allows more efficient dewetting of the liquid bridge from the polymer binder. Although the polymer binder layer is transferred with the part, it can be easily removed afterwards by, for example, oxygen plasma.
[0034] Figure 1A Transferring of components 15 from a donor substrate 10 to an acceptor substrate 20 by irradiating a release stack "S" is shown. In some embodiments, the donor substrate 10 includes a transparent carrier 11 configured to carry the components 15 facing the acceptor substrate 20. Preferably, a release stack "S" is disposed between the transparent carrier 11 and the components 15 for releasing one or more of the components 15 from the donor substrate 10 onto the acceptor substrate 20. Typically, the release is performed directly after the release stack "S" is irradiated by the light beam "L" through the transparent carrier 11.
[0035] In some embodiments, the release stack "S" includes, for example, a melting layer 13 having a relatively low melting temperature "Tm13". In other or additional embodiments, the release stack "S" includes a light absorbing layer 12 disposed between the transparent support 11 and the melting layer 13. In one embodiment, the light absorbing layer 12 has a relatively high absorption coefficient. This can allow the light beam "L" to be efficiently absorbed, thereby causing the light absorbing layer 12 to be heated. In another or additional embodiment, the heated light absorbing layer 12 is in thermal contact with the melting layer 13. This can allow heat to be conducted to the melting layer 13. In this way, the temperature of the melting layer 13 can be raised to above its melting temperature "Tm13". Preferably, the relatively high melting temperature "Tm12" of the light absorbing layer 12 is higher than the melting temperature "Tm13" of the melting layer 13. In this way, the light absorbing layer 12 can remain substantially solid, while the melting layer 13 is substantially melted by the heat conducted from the light absorbing layer 12. In some embodiments, the release stack "S" also includes a decomposition layer 16 located between the light absorbing layer 12 and the melting layer 13. In certain embodiments, the decomposition layer may include a material having an evaporation temperature "Te16" that is higher than the melting temperature "Tm13" of the melting layer 13 and lower than the melting temperature "Tm12" of the light absorbing layer 12. In this way, the decomposition layer 16 may form bubbles 17 when heated above its evaporation temperature "Te16". The bubbles 17 may stimulate or accelerate the release of the component 15, which may be attached to the melting layer 13 by the adhesive layer 14. The formation of the bubbles 17 is not the main driving factor for the release, but only accelerates the release. The release is mainly driven by the melting of the melting layer 13 and the change in adhesion between the layers of the release stack "S" caused by the phase change from solid to liquid, which changes the wetting properties (as further explained below). The bubbles 17 stimulate the release by moving the interface between the melting layer 13 and the decomposition layer 16 and by changing the curvature of the melting layer 13, which in turn stimulates the reduction of the contact area between the melting layer 13 and the underlying layer (e.g., typically the adhesive layer 14). In other or additional embodiments, the release stack "S" includes such an adhesive layer 14 disposed between the component 15 and the melting layer 13. This allows the component 15 to be adhered to the melting layer 13 when the melting layer 13 is solid, and releases the adhesion when the melting layer 13 melts (indicated by "M" in the figure).
[0036] Some embodiments include selectively irradiating a region of the light absorbing layer 12 with a light beam "L" through a transparent carrier 11, forming a portion of a release stack "S" that holds a corresponding component 15. In this way, a corresponding portion of the light absorbing layer 12 can be selectively (locally) heated. Preferably, the heat is conducted to an adjacent melting layer 13 of the release stack "S" via a decomposition layer 16 between the light absorbing layer 12 and the melting layer 13. In this way, the adjacent melting layer 13 can be at least partially melted. Preferably, when the melting layer 13 melts, the corresponding portion of the light absorbing layer 12 remains substantially solid. Advantageously, the melting of the adjacent melting layer 13 may result in a loss of adhesion between the adjacent melting layer 13 and a corresponding portion of the adhesive layer 14 of the release stack "S" that adheres the corresponding component 15 to the adjacent melting layer 13. Therefore, the loss of adhesion may result in the release and transfer of the corresponding component 50. For example, the release allows the component to fall from the donor substrate 10 and / or be pushed to the receptor substrate 20. In the present invention, the release of the component 15 is stimulated by forming bubbles 17 in the decomposition layer 16 between the melting layer 13 and the light absorbing layer 12. The decomposition layer 16 has an evaporation temperature "Te16" that is higher than the melting temperature "Tm13" of the melting layer 13. After the melting layer 13 has melted, the temperature is further increased while energy continues to be added via the light beam "L" for the duration of the light pulse. This causes the decomposition layer to melt and then evaporate when the temperature "Te16" is reached, forming bubbles 17. The formation of bubbles enables the release of the component 15 to be in progress. Although the component 15 is also released in the absence of the decomposition layer 16 in the stack "S", the formation of bubbles 17 advances the release moment and thereby enables the component 15 to receive less heat during the transfer process. Therefore, the component 15 is not susceptible to thermal damage during the transfer process.
[0037] Preferably, the donor substrate 10 is arranged above the acceptor substrate 20 so that gravity can assist the transfer. Alternatively or additionally, the transfer can be induced by a force after irradiation. For example, the release can be induced by melting and / or accompanied by the formation of at least some gas. Aspects of the present disclosure can also be implemented as a system including a donor substrate 10 as described herein. For example, the system includes a light source and / or a controller configured to generate a light beam "L" as described herein.
[0038] In some embodiments, the molten layer 13 includes a metal or is substantially composed of a metal. The inventors have found that the metal molten layer can provide specific benefits for the method and system of the present invention, such as providing a stable connection with various types of adhesive materials and well controlling the release of the adhesive at a predictable melting point. Alternatively or additionally, other molten materials, such as semiconductor materials, alloys, etc., can also be used. Advantageously, for example, for the purpose of the molten layer as described herein, the eutectic alloy can combine the bonding properties of the component metals with the flow properties of the pure metal. In addition, such an alloy can be directly transformed from a solid state to a liquid state at a specific composition and temperature, or vice versa, from a liquid state to a solid state without passing through a two-phase balance. In addition, the eutectic temperature can be much lower than the melting temperature of two or more pure elements. As can be understood, a lower melting temperature "Tm13" is conducive to selecting a material suitable for the decomposition layer 16, because its evaporation temperature "Te16" must be higher than the melting temperature "Tm13" of the molten layer 13 and lower than the melting temperature "Tm12" of the light absorbing layer 12.
[0039] According to other or additional embodiments, the decomposition layer 16 may also be composed of a metal (although there are alternatives). The choice of material also depends on the choice of material for the melting layer 13, since the evaporation temperature "Te16" of the decomposition layer 16 is related to the melting temperature "Tm13" of the melting layer 13. Similarly, the choice of material for the light absorbing layer 12 will also affect the selection of suitable candidate materials for the decomposition layer 16, since the evaporation temperature "Te16" of the decomposition layer 16 must be lower than the melting temperature "Tm12" of the light absorbing layer 12. For example, if aluminum (Al) is to be used for the melting layer 13 and molybdenum (Mb) is to be used as the light absorbing layer 12, the decomposition layer 16 may be made of, for example, silver (Ag), gold (Au) or copper (Cu). For example, in this example, the following table shows the corresponding melting temperatures and evaporation temperatures (at atmospheric pressure):
[0040] Material abbreviation Melting temperature, °C Evaporation temperature, °C molybdenum Mo 2620 5560 aluminum Al 660 2327 copper Cu 1084 2595 gold Au 1063 2600 silver Ag 961 1950
[0041] The above materials are certainly not the only candidates, for example, other metals or alloys, or even non-metals, having the desired properties that can be used for the decomposition layer 16 can be identified. For example, some oxides (Al2O3 and SiO2) have been mentioned before, which have been tested and the results are acceptable. Therefore, the list of candidate materials is certainly not limited to the mentioned materials, but the skilled person knows that the requirements of selection (described above) are considered to be able to identify various candidate materials according to the selection of materials for the melting layer 13 and the light absorbing layer 14. For example, in the case where the melting layer 13 is made of, for example, zinc (Tm≈420°C), tin (Tm≈232°C) and / or indium (Tm≈156°C), other or additional candidates may be found.
[0042] In other or additional embodiments, the light absorbing layer 12 includes a metal or is substantially composed of a metal. The inventors have found that the metal light absorbing layer 12 can provide specific benefits to the methods and systems of the present invention, such as providing relatively good thermal conduction. In addition, the inventors have found that when both the light absorbing layer 12 and the melting layer 13 are metal layers, the molten melting layer 13 may tend to adhere to the light absorbing layer 12 more than to the adhesive layer 14, especially when the adhesive layer 14 is not a metal layer. The same is true for the decomposition layer 16: although the layer is still solid, the molten melting layer 13 may tend to adhere to the decomposition layer 16 more than to the adhesive layer 14. Similarly, when melted and about to evaporate (such as forming bubbles 17), in the case where the light absorbing layer 12 is made of metal (such as Mb), the decomposition layer 16 made of metal (such as silver (Ag)) also adheres well to the light absorbing layer. Similar advantages can also be achieved using a light absorbing layer made of a semiconductor material (such as silicon and silicon carbide).
[0043] In some embodiments, the adhesive layer 14 includes a polymer-based adhesive (preferably a cross-linked polymer, such as an epoxy resin) or is substantially composed of it. Advantageously, polymer adhesives generally have relatively low thermal conductivity compared to metals, so the thermal conductivity to the component 15 can be kept relatively low. In addition, the surface tension of liquid metals is generally much higher than the surface energy of solid polymers. Therefore, the adhesion between the adhesive layer 14 and the molten layer 13 can be released. In contrast, since the surface energy of the solid metal layer is generally relatively high, the metal molten layer 13 can mainly adhere to the metal decomposition layer 16 and the light absorbing layer 12. This means that, in some embodiments, only the polymer part is transferred with the component. Other materials for the adhesive layer can also be envisioned, preferably including organic and / or non-metallic layers or being substantially formed by organic and / or non-metallic layers.
[0044] Regardless of the specific material, the light absorbing layer 12 preferably has a surface energy per unit area (e.g., mJ / m 2) is higher than the adhesive layer 14, for example, at least two times, three times, five times, ten times, twenty times, fifty times or more. The greater the surface energy difference, the more the molten material may tend to adhere to the light absorbing layer 12 rather than the adhesive layer 14. Generally, the surface energy of the molten layer 13 is lower than the light absorbing layer 12, which melts at a lower temperature, and most preferably higher than the adhesive layer 14. In one embodiment, when the molten layer 13 in the release stack "S" of the selected component 15 melts, the molten layer 13 mainly adheres to the decomposed layer 16 (while still solid), and then adheres to the light absorbing layer 12 of the release stack "S", while the adhesive layer 14 of the selected component 15 mainly adheres to the selected component 15. For example, the adhesive layer 14 is transferred to the receptor substrate 20 with the selected component 15, while the molten layer 13 mainly remains with the portion of the release stack "S" on the donor substrate 10. Preferably, the transferred adhesive layer 14 is removed from the selected component 15 after transfer. For example, the polymer adhesive layer 14 can be removed from the component by wet or dry etching. For example, more than fifty percent (preferably more than seventy percent, or even more than ninety percent) of the molten material adheres to the light absorbing layer 12. Most preferably, substantially all of the molten material remains with the stack on the donor substrate 10.
[0045] Figure 1B Various temperatures "T" and sequences for releasing a component 15 by light-induced heating "H" of selected layers in a release stack "S" are shown. Without being bound by theory, the figure shows the duration of the light pulse "Lp", the heat transfer "H13" caused to the melting layer 13, the heat transfer "H14" to the adhesive layer 14, and the resulting melting layer temperature "T13" (arbitrary scale). The following figure shows the various stages of component release. As shown in the figure, the melting layer temperature "T13" generally increases first due to the heat transfer "H13" caused by the light pulse "Lp" irradiating the light absorbing layer. When the melting layer temperature "T13" reaches the melting temperature "Tm13", the increase in temperature may level off, and the energy of the heat transfer "H13" is used for the molten material represented by "M". After the melting layer 13 melts, the temperature rises further and reaches a temperature "Te16". This is the temperature at which one or more bubbles 17 are formed in the decomposition layer 16, thereby stimulating the release and transfer of the component 15. As a further result of the melting of the melting layer 13, the contact between the melting layer 13 and the adhesive layer 14 may decrease and eventually disappear, so even though the heat transfer "H13" to the melting layer 13 may continue, the heat transfer "H14" to the adhesive layer 14 may stop. Advantageously, stopping the heat transfer "H14" to the adhesive layer 14 can mitigate the decomposition of the adhesive layer 14 and / or mitigate damage to the component 15 due to overheating. Therefore, in fact, the melting layer 13 can also act as a buffer layer to protect the component 15 from damage.
[0046] In some embodiments, the relatively low melting temperature "Tm13" of the melting layer 13 is less than one thousand degrees Kelvin (<~700°C), preferably less than six hundred degrees Kelvin (<~300°C). The lower the melting temperature of the melting layer 13, the less energy is required for melting, for example, allowing a lower intensity light beam "L" and / or less chance of damaging parts. For example, suitable materials for the melting layer may include aluminum (Tm≈660°C), zinc (Tm≈420°C), tin (Tm~232°C) and / or indium (Tm≈156°C).
[0047] In other or additional embodiments, in the case of a non-melting material of the light absorbing layer 12, the melting temperature "Tm12" or the decomposition / evaporation temperature is higher than the melting temperature "Tm13" of the melting layer 13. In addition, in the case of a non-melting material of the light absorbing layer 12, the melting temperature "Tm12" or the decomposition / evaporation temperature is also higher than the evaporation temperature "Te16" of the decomposition layer 16, for example at least ten degrees Kelvin, preferably at least fifty degrees Kelvin, more preferably at least one hundred degrees Kelvin, most preferably at least two hundred degrees Kelvin, or even more than five hundred degrees Kelvin. The greater the difference between the melting temperature Tm13 and the evaporation temperature Tm16 on the one hand and the melting temperature Tm12 on the other hand, the easier it is to ensure that the light absorbing layer 12 remains substantially solid, while the melting layer 13 is at least partially melted and bubbles are formed in the decomposition layer by heat conducted from the light absorbing layer 12. Preferably, the melting temperature "Tm12" or the decomposition / evaporation temperature for non-melting materials is at least one thousand degrees Kelvin ≥ ~ 700 ° C, more preferably at least two thousand degrees Kelvin. Particularly suitable metals for use in the light absorbing layer 12 include molybdenum, which has a relatively high melting temperature of 2896K (2623°C). Other metals with relatively high melting temperatures, such as chromium (2180K, 1907°C), may also be used. As an alternative to metals, other materials may also be used for the light absorbing layer 12, such as semiconductor materials or other materials that can conduct heat to the melting layer 13 while remaining solid, preferably with a relatively high absorptivity to the light beam "L". In some embodiments, a wetting control layer 12w may be disposed between the (main) light absorbing layer 12 and the melting layer 13. For example, suitable materials for the wetting control layer 12w may include oxides, such as aluminum oxide or silicon oxide. Since these materials also provide viable alternatives to the decomposition layer 16, embodiments including a thin layer of aluminum oxide or silicon oxide provide a decomposition layer 16 with dual functionality, which may be beneficial in certain applications.
[0048] In some embodiments, the light beam "L" irradiating the release stack "S" is configured to raise the temperature "T13" of the molten layer 13 to above its melting temperature "Tm13" but keep it below its evaporation temperature Te13. For example, the intensity and / or duration of the light beam "L" are adapted to be related to the absorptivity of the light absorbing layer 12 so that a specific amount of energy of the light beam "L" is deposited in the light absorbing layer 12, causing a specific increase in the temperature of the light absorbing layer 12, and transferring a specific amount of heat to the molten layer 13, which is sufficient to melt the molten layer 13, but not enough to cause substantial boiling and / or evaporation of the molten layer 13. The more the evaporation of the molten layer 13 can be prevented, the more the release of the component 15 can be controlled. For example, the explosive release of the component can be mitigated. Advantageously, the evaporation or boiling temperature of the molten layer can be much higher than its melting temperature, especially for metal molten layers. For example, the evaporation temperature Te13 of the molten layer 13 is at least five hundred degrees Kelvin higher than its melting temperature "Tm13", preferably at least one thousand degrees Kelvin, or even more than one thousand five hundred degrees Kelvin. The greater the difference between the melting temperature and the evaporation temperature, the easier it is to prevent evaporation of the molten layer.
[0049] In some embodiments, the adhesive layer 14 has a decomposition temperature Td14 that is higher than the melting temperature "Tm13" of the melting layer 13 [Td14>Tm13], or at least within five hundred degrees Kelvin below the melting temperature "Tm13" of the melting layer 13 (higher than five hundred degrees Kelvin) [Td14>(Tm13-500K)], preferably within four hundred degrees Kelvin, or within three hundred degrees Kelvin. The higher the evaporation or decomposition temperature Td14 of the adhesive layer 14, the more it can prevent accidental decomposition and obtain a more controlled release of the component 15. It should be noted that the decomposition temperature Td14 of the adhesive layer 14 is generally suitable for long-term exposure to this temperature. Therefore, brief exposure of the adhesive layer 14 to a temperature above the decomposition temperature Td14 of the adjacent melting layer 13 can be tolerated, also because the molten material tends to adhere to the light absorbing layer 12 and / or dewet from the adhesive layer 14. For example, suitable materials for the adhesive layer may include photoresist materials such as SU-8. Other materials, such as polyimide, may also be used.
[0050] As a non-limiting example, consider the approximate parameters in the following table.
[0051]
[0052]
[0053] In some embodiments, the light beam "L" irradiating the release stack "S" is provided as a relatively short light pulse, for example having a FWHM duration of less than one millisecond (preferably less than one hundred nanoseconds, more preferably less than ten nanoseconds, or even less than one nanosecond). For example, the light can be provided as nanosecond or picosecond pulses. The shorter the light pulse, the higher the intensity per unit time of the pulse duration. This may cause a relatively short and intense heating of the stack, and preferably melt the components before thermally decomposing the adhesive layer 14 and / or before thermally damaging the components 15.
[0054] In some embodiments, the light absorbing layer 12 is configured to absorb at least 10 percent, preferably at least 20 percent, more preferably at least 50 percent or 60 percent, and most preferably at least 90 percent of the light beam "L" irradiating the release stack "S". For example, the light beam "L" has a wavelength between 100 nm and 2000 nm (e.g., monochromatic or broadband light), preferably NIR laser (e.g., 1064 nm). Other wavelengths, such as UV, visible light, or infrared, may also be used, as long as the material of the light absorbing layer 12 can fully absorb the wavelength.
[0055] In some embodiments, the light beam "L" is configured to illuminate only a sub-region of the light absorbing layer 12 that forms a portion of the selected release stack "S" that holds the selected component 15, while not illuminating the immediately adjacent region of the light absorbing layer 12, thereby releasing only the selected component 15 while the adjacent component remains attached to the donor substrate 10. For example, the light beam "L" has a beam width "WL" that is approximately equal to or less than the width "W15" of the selected component, and / or the light beam "L" is centered on the selected component. In one embodiment, a light beam "L" having a relatively narrow beam width is generated that illuminates one or more sub-regions of the release stack "S" corresponding to one or more components. In another or additional embodiment, the light beam "L" is focused to a relatively narrow beam width, such as using one or more lenses / reflectors to project a relatively small spot onto one or more sub-regions of the release stack "S". In another or additional embodiment, the relatively wide light beam "L" is shaped or patterned, such as using a mask pattern, to generate one or more relatively narrow beams that illuminate one or more sub-regions of the release stack "S". In one embodiment, the light beam "L" is generated by a laser, for example, to illuminate a specific feature or portion of a mask pattern. Other light sources may also be used, such as a flash lamp that illuminates a portion of the mask pattern or the entire mask.
[0056] Figure 2A and Figure 2BOther aspects are shown including cutting and / or etching portions of the release stack "S". In some embodiments, the release stack "S" is at least partially segmented or diced (in the projection view), for example, along lanes or cut lines "C" between and / or around the components 15. For example, one or more layers of the stack may be segmented before or after the components are connected (preferably at least before the transfer). Preferably, at least the adhesive layer 14 is segmented so that portions of the adhesive layer 14 that hold different components 15 are separated from each other. In this way, the transfer of the individual components 15 can be better controlled while reducing interference with intermediate pieces of the adhesive layer 14. More preferably, the melting layer 13 is also segmented so that portions of the melting layer 13 corresponding to different components 15 are separated from each other. In this way, the molten material of the release component can be kept separate from the melting layer 13 of the adjacent component, for example to prevent interference with the component released later. More preferably, the decomposition layer 16 is also segmented so that portions of the decomposition layer 16 corresponding to different components 15 are separated from each other. In this way, bubbles 17 formed in the decomposed layer 16 when reaching its evaporation temperature Tm16 will be self-limited within the patch below the component 15 to be separated. This prevents the accidental loss of adjacent components 15 during transfer. More preferably, the light absorbing layer 12 is also segmented so that the parts of the light absorbing layer 12 corresponding to different components 15 are separated from each other. In this way, the heating of the light absorbing layer 12 can be better kept localized and / or prevent heat transfer to adjacent areas of the light absorbing layer 12 corresponding to adjacent components. This can also facilitate aiming the laser at the component from the back side.
[0057] In some embodiments, for example, Figure 2BAs shown, at least a portion of the molten layer 13 is removed to provide a corresponding undercut between the component 15 and the donor substrate 10. In one embodiment, the area of the molten layer 13 that maintains the corresponding component 15 is smaller than the area of the corresponding component, for example, at least two times, three times, four times, five times or more. By providing a relatively small area of the molten layer 13, the material can be more easily melted to release the component without melting the adjacent portion of the molten layer 13. Preferably, the smaller area is still centered on the corresponding component, for example, to alleviate the rotation of the component during transfer. In connection with this, and according to some of these embodiments, the thin decomposition layer 16 can also have a size similar to the molten layer 13, as shown. Due to the surface tension of the light absorbing layer 12, the self-limiting bubbles 17 formed by the decomposition layer 16 reaching the evaporation temperature Te16 will remain adhered to the surface of the light absorbing layer. In another or additional embodiment (not shown), the adhesive layer 14 can also have a smaller area, for example, so that less material needs to be removed later. In another or additional embodiment not shown, the light absorbing layer 12 can also have a smaller area to further improve the thermal separation from the adjacent components. For example, portions of the molten layer 13 and / or other layers may be removed beneath the component by etching as indicated by "E". In other or additional embodiments, the width "WL" of the beam "L" is less than the width "W15" of the corresponding component 15 being released. For example, the area or width "WL" of the beam "L" may be adjusted to the area of the molten layer 13.
[0058] Figure 3A A mask of light pulses "Lp" is shown to form a relatively narrow beam L and the relative thickness of each layer. In some embodiments, the mask 30 is aligned with the donor substrate 10. In one embodiment, the mask 30 includes a set of mask windows (open areas) aligned with a subset of features 15 on the donor substrate 10. In another or additional embodiment, a set of light spots (e.g., light pulses Lp) are used to illuminate the set of mask windows sequentially or simultaneously. In another or additional embodiment, the corresponding light spot (e.g., laser spot) is larger than the corresponding mask window (which is illuminated, and the light spot is preferably centered on the window), for example, the full width half maximum (FWHM) spot size (diameter) is at least two, three or more times larger than the width of the mask window, but is small enough, such as four or five times smaller, so that the tail of the spot does not substantially illuminate another mask window. Typically, the laser spot has a Gaussian intensity distribution. By masking the spot so that only the central portion of the spot passes through the mask window, the intensity distribution can be relatively flat, which may be conducive to controlled release.
[0059] Preferably, the transparent carrier 11 of the donor substrate 10 is formed of a relatively thin foil, for example, having a thickness "Ds" of less than two millimeters or even less than one millimeter. The thinner the transparent carrier, the easier it is to illuminate the stack through it (for example, with a mask). For example, the donor substrate 10 can be a flexible or rigid substrate. Typically, the component is very small, for example, having a thickness "Dc", height or other cross-sectional dimensions of less than one hundred microns, less than fifty microns or even less than thirty microns. Typically, the release stack "S" has a much smaller thickness "Dr", for example, less than ten microns or even less than one micron. Preferably, the component 15 is transferred from the donor substrate 10 to the receptor substrate 20 without contact, for example, within a transfer distance "Dt" between one micron and one hundred microns (preferably between twenty microns and sixty microns). These ranges can provide sufficient distance to prevent unintentional contact on the one hand, and are close enough to allow controlled transfer on the other hand. Alternatively, other distances can also be used. In some embodiments, preferably, the transfer distance is greater than the thickness of the component, so that the technology can also be used for repair purposes.
[0060] In one embodiment, the light absorbing layer 12 has a layer thickness of less than 500nm, preferably less than 250nm, for example, between 50nm and 150nm. Providing a relatively thin light absorbing layer 12 can allow the layer to be heated relatively quickly. On the other hand, the layer may require a certain thickness to absorb light. In another or additional embodiment, the melting layer 13 has a layer thickness of less than 500nm, preferably less than 250nm, for example, between 50nm and 150nm. Providing a relatively thin melting layer 13 can allow the layer to be heated and melted relatively quickly. On the other hand, the layer may require a certain thickness to provide its function. In another or additional embodiment, the melting layer 13 has a layer thickness of less than one micron, for example, between 50nm and 500nm. According to another or additional embodiment, the decomposition layer 16 should preferably be thinner than the melting layer 13. The reason for doing this is that after the melting layer 13 reaches the liquid phase, it should preferably be heated relatively quickly, and in addition, the heat conduction from the light absorbing layer 12 to the melting layer 13 should remain efficient. Therefore, the decomposition layer 16 can preferably be five to twenty times thinner than the melting layer 13. However, there is also a lower limit to the thickness, because the layer needs to be thick enough to melt and form bubbles 17. Therefore, the decomposition layer 16 can generally have a thickness of the order of tens of nanometers; in order to give a numerical range, the thickness of the decomposition layer 16 can be between 5 nanometers and 100 nanometers, preferably between 5 nanometers and 50 nanometers. In addition, in principle, the thinner the adhesive layer 14, the less material needs to be cleaned later (if it is really needed). On the other hand, depending on its function, the layer may need a certain thickness, for example greater than 250nm. Other layer thicknesses can also be used.
[0061] As a non-limiting example, the donor substrate is prepared as follows. Starting from a clean quartz / glass transparent carrier, a 130nm light absorbing layer of molybdenum is sputtered onto the carrier. A molten layer of 120nm aluminum is sputtered onto the previous layer. A 500nm SU-8 adhesive layer is spin-coated onto the previous layer. The carrier and stack are soft-baked at 95°C for 2 minutes. The components are vacuum laminated to the carrier / stack at 120°C for 15 minutes. The temporary polymer tape is removed from the components. Oxygen plasma is applied at 500W for 1 hour to remove the SU-8 between the components. Aluminum and molybdenum are etched in PES etchant 77-23-04 for 2 minutes. The SU-8 resist is hard-baked at 250°C for 3 hours. Of course, other materials, layer thicknesses, temperatures, etc. can also be used.
[0062] In some embodiments, the mask 30 is formed of a pattern of light absorbing material disposed on a transparent carrier, forming a corresponding mask window that can be aligned with the portion of the release stack "S" that holds the corresponding component 15. As a non-limiting example, the mask substrate is prepared as follows. Starting with a clean quartz / glass transparent carrier, a 130nm molybdenum light absorbing layer is sputtered onto the carrier. 2pm of HPR504 resist is spin coated onto the light absorbing layer. The stack is soft baked at 95°C for 2 minutes. The resist is selectively irradiated according to the mask pattern. HPR504 resist is under development. HPR504 resist is hard baked at 120°C for 2 minutes. Molybdenum is etched in PS etchant for 30 seconds. The HPR504 resist is removed by micro-peeling. Clean the mask substrate. Advantageously, the mask 30 can use a light absorbing material that is the same or similar to the light absorbing layer 12 in the release stack "S". Other materials such as a standard chrome-coated quartz mask can also be used, since chrome melts at 1907°C and will not be damaged by the flux and laser power of the molten aluminum layer.
[0063] Figure 3B 1 shows a sequential release of components 15. In some embodiments, components are released from donor substrate 10 according to a particular sequence, wherein at least some components, preferably most components, and most preferably each component 15 have four directly adjacent neighboring components on all sides (e.g., Figure 3B ), or have no directly adjacent neighboring components on any side (such as Figure 3B). In one embodiment, combinations may also be used, for example, having two directly adjacent adjacent components on a first set of two opposing sides and no directly adjacent components on a second set of opposing sides (not shown). For example, the non-existent adjacent components may not initially exist, or may be released when they are surrounded by components that are still present. By balancing the presence or absence of directly adjacent adjacent components on opposing sides, the components may be released in a more balanced manner, for example allowing gas generation of the adhesive layer to push the components away in a controlled directionality. For example, the components may be released according to a checkerboard pattern as shown. Other patterns may also be envisioned. Furthermore, it will be understood that while the release sequence provides particular advantages in conjunction with the particular release stacks described herein, the sequence may in principle be advantageous for light-induced transfer of components using any type of release stack, particularly where gas generation in the stack is involved when the components are released.
[0064] Figure 4A A photograph of a feature 15 transferred to a receptor substrate 20 using the methods described herein is shown. In this case, the transferred feature is 40 x 40 μm 2 The chip has a pixel pitch of 200pm. Figure 4B This is a photograph in which the surface of the air bubble 17 remains present on the surface of the light absorbing layer 12 after the component 15 has been transferred. The convex curvature of the surface is very obvious. Figure 4C A portion of the remaining stack S' on the donor substrate 10 is shown. In this case, molten aluminum on the molybdenum is visible after part transfer. As shown, the width "Ws" of the remaining stack is about 15 μm, for example, smaller than the transferred part.
[0065] Figure 5AAn embodiment is shown in which the donor substrate 10 (e.g., stack "S") includes a thermal insulation layer 11i located between the transparent carrier 11 and the light absorbing layer 12. Therefore, both the thermal insulation layer 11i and the light absorbing layer 12 can be disposed between the transparent carrier 11 and the melting layer 13. In some embodiments, the thermal insulation layer 11i has a relatively low thermal conductivity, such as lower than the thermal conductivity of the material forming the transparent carrier 11. In other or additional embodiments, the thermal insulation layer 11i has a relatively high transparency (for the light beam "L"), such as higher than the material forming the light absorbing layer 12. Advantageously, the relatively transparent thermal insulation can allow the light beam "L" to pass through from the transparent carrier 11 to illuminate and heat the light absorbing layer 12, while preventing or at least reducing heat transfer from the light absorbing layer 12 back to the transparent carrier 11. In this way, heat can be transferred to the melting layer 13 more efficiently. In one embodiment, for example, as shown, the thermal insulation layer 11i is segmented between components 15. This can further reduce heat transfer back to the transparent carrier 11 and / or reduce heat transfer between adjacent components. It will be appreciated that while the thermal insulation layer 11i is shown here with a specific embodiment, the layer may also be used in conjunction with any other embodiment as described herein (segmented or unsegmented).
[0066] Figure 5BAn embodiment is shown in which the donor substrate 10 (e.g., stack "S") includes a dewetting layer 12d located between the decomposition layer 16 and the melting layer 13. In general, dewetting describes the process of a fluid withdrawing from a surface it is forced to cover, in this case, the molten material "M" of the melting layer 13 withdrawing from the dewetting layer 12d. One factor that describes the spontaneous diffusion and dewetting of a drop of liquid on a surface solid (e.g., with an ambient gas) is the so-called diffusion coefficient "S". Spontaneous diffusion occurs when S>0, and if S<0, partial wetting or dewetting may be observed. Alternatively or additionally, wetting and dewetting can be described by the equilibrium contact angle θc of a drop of liquid on the surface. When the surface is more wet, the contact angle may be smaller; and when the surface is more dewetting, the contact angle may be smaller. In some embodiments, the dewetting layer 12d is applied to promote the dewetting of the molten material "M" of the melting layer 13 compared to the light absorbing layer 12. For example, the molten material "M" on the dewetting layer 12d has a lower diffusion coefficient and / or a higher equilibrium contact angle than the molten material "M" on the light absorbing layer 12. Controlled dewetting can have various advantages, such as retracting the molten material "M", which can improve the release adhesion of the selected component 15. Retraction can also help push the selected component through local accumulation of material. Preferably, the dewetting layer 12d has a melting temperature higher than the melting temperature of the melting layer 13, and may also be higher than or equivalent to the melting temperature of the decomposition layer 16. Preferably, the dewetting layer 12d has relatively good thermal conductivity and / or is relatively thin, so that the heat transfer from the light absorbing layer 12 to the melting layer 13 is minimally affected, or not affected at all. For example, compared with the light absorbing layer 12, the dewetting layer 12d can have the same, similar or higher thermal conductivity. In some embodiments, the dewetting layer 12d is formed by a (thin) coating (e.g., a single layer) on the decomposition layer 16. Therefore, the heated light absorbing layer 12 can be in thermal contact with the melting layer 13 via the decomposition layer 16 and the dewetting layer 12d. In the case where the materials of the decomposition layer 16 and the dewetting layer 12d meet the requirements of the two layers, they can be combined into a single functional layer. For example, the possibility of using aluminum oxide or silicon oxide as a candidate for a layer for providing the two functions of the above-mentioned layers 16 and 12d has been proposed above.
[0067] Figure 6The release of the component 15 from the donor substrate 10 is shown by irradiating the release stack S with a plurality of light pulses, as described in the above embodiments. Some embodiments include irradiating a corresponding region of a light absorbing layer forming a portion of a corresponding release stack holding the corresponding component with a first light pulse L1 to heat the corresponding portion of the light absorbing layer and initiate and / or complete melting of an adjacent portion of the molten layer. Other or additional embodiments include irradiating a corresponding region of the light absorbing layer with a second light pulse L2 to further promote the release of the component 15 from the partially or completely melted material "M" of the molten layer 13. In one embodiment, the first light pulse L1 is relatively long, for example, long enough to completely melt the molten layer 13, as shown. In another or additional embodiment, the molten layer 13 can be at least partially melted by the first light pulse L1. In another or additional embodiment, the second light pulse L2 is relatively short and / or has a relatively high power compared to the first light pulse L1. In some embodiments, the first light pulse L1 causes a relatively gradual melting of the molten layer 13, for example, having a pulse length of more>1ns,>10ns,>100ns or even>1μs. In other or additional embodiments, the second light pulse L2 causes a relatively high heat flux, for example having a pulse length of <1μs, <100ns, <10ns, <1ns, <100ps or even less. For example, a sudden high heat flux can also promote the release of the component 15 from the partially or completely molten material "M". For example, the second light pulse L2 can cause the formation of bubbles 17 by rapidly heating the decomposition layer 16 to above its evaporation temperature Te16. It can also further cause shock waves in the molten material and / or at least partial decomposition of the adhesive layer 14. In some embodiments, the first light pulse L1 causes a reduction in the contact area of the molten material, for example by dewetting on the light absorbing layer or the optional dewetting layer. In some embodiments, the second light pulse L2 generates gas, for example by decomposition or other means, causing a final push to release the component. Although the present figure shows two separate light pulses, other or additional embodiments can use a single modulated light pulse to achieve a similar effect, such as increasing the power at the end of the pulse. It is also conceivable to use more than two pulses. In some embodiments, for example, as shown in the figure, the decomposition temperature Td14 of the adhesive layer 14 is higher than the melting temperature Tm13 of the melting layer 13. In other embodiments, for example, Figure 1B As shown and described with reference thereto, this may also be reversed [eg within a certain range such as Td14>(Tm13-300K)].
[0068] In interpreting the appended claims, it should be understood that the word "comprising" does not exclude the presence of other elements or actions than those listed in a given claim; the word "a" or "an" preceding an element does not exclude the presence of a plurality of such elements; any reference signs in the claims do not limit their scope; and unless otherwise specifically stated, any device or part thereof disclosed may be combined together or separated into other parts.
Claims
1. A method for light-induced transfer of a component (15) from a donor substrate (10) to a receptor substrate (20), wherein: The donor substrate (10) comprises: a transparent carrier (11) configured to carry the component (15) facing the receptor substrate (20), and a release stack (S) disposed between the transparent carrier (11) and the components (15), for releasing one or more of the components (15) from the donor substrate (10) onto the receptor substrate (20) after the light beam (L) is irradiated onto the release stack (S) through the transparent carrier (11), wherein the release stack (S) comprises: a melting layer (13) having a melting temperature (Tm13), A light absorbing layer (12) is arranged between the transparent carrier (11) and the melting layer (13), wherein the light absorbing layer (12) has an absorption coefficient for absorbing the light beam (L) so that the light absorbing layer (12) is heated, wherein the heated light absorbing layer (12) is in thermal contact with the melting layer (13) to conduct the heat of the light absorbing layer to the melting layer (13), thereby raising the temperature of the melting layer (13) to above the melting temperature (Tm13) of the melting layer, wherein: The light absorbing layer (12) has a melting temperature (Tm12) higher than the melting temperature (Tm13) of the melting layer (13), so that when the melting layer (13) is melted by heat conducted from the light absorbing layer (12), the light absorbing layer (12) can remain solid, a decomposition layer (16) disposed between the melting layer (13) and the light absorbing layer (12), wherein the decomposition layer (16) has an evaporation temperature (Te16) higher than a melting temperature (Tm13) of the melting layer and lower than a melting temperature (Tm12) of the light absorbing layer (13), and wherein a layer thickness of the decomposition layer (16) is smaller than a layer thickness of the melting layer (13); and an adhesive layer (14) for adhering the component (15) to the molten layer (13) when the molten layer (13) is solid, and for releasing the adhesive force when the molten layer (13) melts (M); The method comprises: irradiating a region of the light absorbing layer (12) through the transparent carrier (11) with a light beam (L) to form a portion of the release stack (S) holding a corresponding component (15) to heat the corresponding portion of the light absorbing layer (12), wherein the heat is conducted to the melting layer (13) of the release stack (S) via the decomposition layer (16), thereby melting the melting layer (13) and heating the decomposition layer (16) while the corresponding portion of the light absorbing layer (12) remains solid, wherein the melting layer (13) The melting of the decomposition layer (16) causes a loss of adhesion between the molten layer (13) and the corresponding portion of the adhesive layer (14) of the release stack (S), the adhesive layer adhering the corresponding component (15) to the molten layer (13), wherein the loss of adhesion causes the release and transfer of the corresponding component (50), and wherein the heating of the decomposition layer (16) causes local gas generation, thereby forming bubbles in the decomposition layer (16), thereby accelerating the loss of adhesion between the molten layer (13) and the corresponding portion of the adhesive layer (14).
2. The method according to claim 1, wherein: The decomposition layer (16) has a melting temperature (Tm16) higher than the melting temperature (Tm13) of the melting layer (13).
3. The method according to any one of claims 1 or 2, wherein: The layer thickness of the decomposition layer (16) is less than 20% of the thickness of the molten layer, preferably less than 15% of the thickness of the molten layer; more preferably less than 10% of the thickness of the molten layer.
4. A method according to any one of the preceding claims, wherein: The layer thickness of the decomposition layer (16) is between 5 nm and 100 nm, preferably between 5 nm and 50 nm.
5. A method according to any one of the preceding claims, wherein: One or more of the following: The molten layer (13) comprises a first metal layer; The light absorbing layer (12) comprises a second metal layer; and / or The decomposition layer (16) includes a third metal.
6. A method according to any one of the preceding claims, wherein: At least one of the following: The decomposition layer has an evaporation temperature (Te16) lower than the evaporation temperature (Te13) of the molten layer; or The decomposition layer has an evaporation temperature (Te16) that is at most 15% higher than the evaporation temperature (Te13) of the molten layer.
7. A method according to any one of the preceding claims, wherein: The light beam (L) irradiating the release stack (S) is configured to: The temperature (T13) of the molten layer (13) is raised to a temperature above the melting temperature (Tm13) of the molten layer but maintained below the evaporation temperature (Te13) of the molten layer, and further, After the temperature (T13) of the melting layer (13) has been raised to above the melting temperature (Tm13), the temperature (T16) of the decomposition layer (16) is raised to above the evaporation temperature (Te16) of the decomposition layer.
8. A method according to any one of the preceding claims, wherein: The adhesive layer (14) has a decomposition temperature (Td14) higher than the melting temperature (Tm13) of the melting layer (13), or higher than three hundred degrees Kelvin below the melting temperature (Tm13) of the melting layer (13).
9. A method according to any one of the preceding claims, wherein: At least one of the adhesive layer (14), the melting layer (13), the decomposition layer (16) and the light absorbing layer (12) is segmented between the components (15).
10. A method according to any one of the preceding claims, wherein: The area of the molten layer (13) holding the corresponding component (15) is at least two times smaller than the area of the corresponding component.
11. A method according to any one of the preceding claims, wherein: A mask (30) is aligned with the donor substrate (10), wherein the mask (30) comprises a set of mask windows aligned with a subset of the components (15) on the donor substrate (10), wherein a set of light spots is used to sequentially or simultaneously illuminate the set of mask windows for releasing corresponding components (15), wherein a corresponding light spot is larger than the corresponding mask window being illuminated, wherein the light spot FWHM diameter is at least twice greater than the width of the mask window.
12. A method according to any one of the preceding claims, wherein: The light absorbing layer (12) is configured to absorb at least fifty percent of the light beam (L) irradiating the release stack (S), wherein the light beam (L) is configured to irradiate only a sub-region of the light absorbing layer (12) that forms a portion of the selected release stack (S) that retains the selected component (15), without irradiating adjacent areas of the light absorbing layer (12), thereby releasing only the selected component (15) while adjacent components remain attached to the donor substrate (10).
13. A method according to any one of the preceding claims, wherein: The melting temperature (Tm13) of the melting layer (13) is less than six hundred degrees Kelvin, wherein the melting temperature (Tm12) of the light absorbing layer (12) is at least one hundred degrees Kelvin higher than the melting temperature (Tm13) of the melting layer (13).
14. A donor substrate (10), comprising: A transparent carrier (11) carrying components (15) for light-induced transfer, and a release stack (S) disposed between the transparent carrier (11) and the components (15) for releasing one or more of the components (15) from the donor substrate (10) after the release stack (S) is irradiated by a light beam (L) through the transparent carrier (11), wherein the release stack (S) comprises: The melting layer (13) has a relatively low melting temperature (Tm13), A light absorbing layer (12) is arranged between the transparent carrier (11) and the melting layer (13), wherein the light absorbing layer (12) has a relatively high absorption coefficient for absorbing at least fifty percent of a light beam (L) having a wavelength range between 100 nm and 2000 nm and a pulse length less than ten nanoseconds, thereby heating the light absorbing layer (12), wherein the light absorbing layer (12) is in thermal contact with the melting layer (13) to conduct its heat to the melting layer (13), thereby raising the temperature of the melting layer (13) to above the melting temperature (Tm13) of the melting layer, wherein the light absorbing layer (12) has a relatively high melting temperature (Tm12) higher than the melting temperature (Tm13) of the melting layer (13), so that when the melting layer (13) is melted by the heat conducted from the light absorbing layer (12), the light absorbing layer (12) can remain solid, and a decomposition layer (16) disposed between the melting layer (13) and the light absorbing layer (12), wherein the decomposition layer (16) has an evaporation temperature (Te16) higher than a melting temperature (Tm13) of the melting layer and lower than a melting temperature (Tm12) of the light absorbing layer (13), and wherein a layer thickness of the decomposition layer (16) is smaller than a layer thickness of the melting layer (13); An adhesive layer (14) adheres the component (15) to the molten layer (13) when the molten layer (13) is solid, and releases the adhesive force when the molten layer (13) melts (M).
15. A system for light-induced transfer of a component (15), the system comprising: The donor substrate (10) according to the preceding claim, comprising: a transparent support (11) and a release stack (S), the release stack having a light absorbing layer (12), a melting layer (13) and an adhesive layer (14) for holding the components (15), wherein the adhesive layer (14) is segmented between the components (15); a receptor substrate (20); and A controller and a light source, the light source being configured to generate a light beam (L) to illuminate a region of the light absorbing layer (12) through the transparent carrier (11) to form a portion of the release stack (S) holding a corresponding component (15) to heat the corresponding portion of the light absorbing layer (12), wherein the heat is conducted to the melting layer (13) of the release stack (S) via the decomposition layer (16), thereby melting the melting layer (13) and heating the decomposition layer (16) while the corresponding portion of the light absorbing layer (12) remains solid, wherein the melting layer (13) 3) causes a loss of adhesion between the molten layer (13) and the corresponding portion of the adhesive layer (14) of the release stack (S), the adhesive layer adhering the corresponding component (15) to the molten layer (13), wherein the loss of adhesion causes the release and transfer of the corresponding component (50), and wherein the heating of the decomposition layer (16) causes local gas generation, thereby forming bubbles in the decomposition layer (16), thereby accelerating the loss of adhesion between the molten layer (13) and the corresponding portion of the adhesive layer (14).