High-activity thermoplastic polyurethane bone repair membrane as well as preparation method and application thereof
By electrospinning the borosilicate-based bioactive glass microspheres doped with thermoplastic polyurethane and selenium, the shortcomings of existing bone repair materials in terms of biological activity, mechanical properties and degradation rate are solved, and the results are achieved. Excellent biocompatibility and antibacterial properties, suitable for bone repair materials.
Patent Information
- Application Number
- CN202411106617.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-06
AI Technical Summary
The existing bone repair materials have defects in bioactivity, mechanical properties, biocompatibility and degradation rate, and lack antibacterial properties, making it difficult to fit the bone defect surface after implantation and induce new bone formation.
Using a highly reactive thermoplastic polyurethane bone repair film, prepared by mixing thermoplastic polyurethane and selenium-doped borosilicate-based bioactive glass microspheres, made by electrospinning technology, combined with N,N-dimethylformamide solution Treatment to form a bone repair membrane with excellent biological activity, mechanical properties and antibacterial properties.
It achieves excellent biological activity, good mechanical properties and orderly and controllable degradation properties of the material, improves osteoblast activity, enhances antibacterial properties, and is suitable for the field of bone repair materials.
Smart Images

Figure CN119074996A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomaterials, and specifically relates to a highly active thermoplastic polyurethane bone repair membrane and a preparation method and application thereof. Background Art
[0002] At present, hard tissue injury is still one of the diseases that people of different ages may suffer from, which makes the market have a huge demand for bone repair and bone replacement materials that can guide rapid bone recovery every year. Among the third-generation artificial bone repair and replacement materials, bioactive glass has attracted widespread attention due to its high controllability of structure, morphology and components. In addition, adding therapeutic ions to bioactive glass can adjust the material properties and promote tissue repair together. However, the brittleness and rapid degradation rate of bioactive glass limit its application in bone repair materials. In order to make up for the unsatisfactory defects in mechanical properties and degradation rate, it is a more feasible method to prepare artificial bone repair materials by compounding bioactive glass with polymers.
[0003] At present, the bone tissue engineering materials that are widely used in clinical practice have certain defects. The main problem is that the materials used for bone repair are difficult to achieve ideal bone union after implantation into the human body due to insufficient biological activity, poor mechanical properties and biocompatibility. In addition, some bone repair membrane materials are synthesized with artificially synthesized high molecular weight polylactic acid and other materials, which will produce acidic substances during the degradation process, which are toxic to surrounding tissue cells, and there is also the problem that the degradation rate is difficult to control. Furthermore, due to the lack of certain antibacterial properties of the materials, bacterial infection and inflammation caused by the implantation of the materials is also a more serious problem.
[0004] Therefore, the existing technology has at least poor biological activity, mechanical properties, and biocompatibility, difficult to control degradation rate and tissue acid-base environment, lack of certain antibacterial properties, which makes it unfavorable for implantation or fails to better fit the bone defect surface and induce new bone formation after implantation. Summary of the invention
[0005] In order to overcome the deficiencies of the prior art, the present invention provides a highly active thermoplastic polyurethane bone repair membrane and a preparation method and application thereof.
[0006] The technical solution of the present invention is:
[0007] 1. A highly active thermoplastic polyurethane bone repair membrane
[0008] The repair film is mainly prepared by mixing thermoplastic polyurethane as an organic component and borosilicate-based bioactive glass microspheres as selenium-doped inorganic components.
[0009] The molecular weight of the thermoplastic polyurethane is 80,000 to 100,000, and the mass percentage concentration is 10 to 20 wt%;
[0010] The diameter of the bioactive glass microspheres is 160-320 nm. The components of the bioactive glass microspheres include silicon dioxide, calcium oxide, phosphorus pentoxide, boron trioxide and selenium dioxide, and the molar ratio of the components is (0-50): (30-36): (4-5): (10-60): (0-5).
[0011] Typically, the components of the bioactive glass microspheres can be one of the following:
[0012] The first type comprises silicon dioxide, calcium oxide, phosphorus pentoxide, boron trioxide and selenium dioxide, and the molar ratio of the components is (0.01-50): (30-36): (4-5): (10-60): (0.01-5);
[0013] The second type includes calcium oxide, phosphorus pentoxide, and boron trioxide, and the molar ratio of the components is (30-36): (4-5): (10-60);
[0014] The third type includes silicon dioxide, calcium oxide, phosphorus pentoxide, and boron trioxide, and the molar ratio of the components is (0.01-50): (30-36): (4-5): (10-60);
[0015] The fourth type includes calcium oxide, phosphorus pentoxide, boron trioxide and selenium dioxide, and the molar ratio of the components is (30-36): (4-5): (10-60): (0.01-5).
[0016] The mass ratio of the bioactive glass microspheres to the thermoplastic polyurethane particles is (1-7):100.
[0017] 2. Preparation method of a highly active thermoplastic polyurethane bone repair membrane
[0018] The preparation method comprises the following steps:
[0019] 1) mixing the template solution and the catalyst solution, and then adding a precursor substance thereto at intervals, adding a different precursor substance each time, and sequentially stirring, aging, centrifuging, washing, drying and calcining to obtain bioactive glass microspheres;
[0020] 2) The bioactive glass microspheres prepared in step 1) are dispersed and added into N,N-dimethylformamide solution, and then thermoplastic polyurethane particles are added and stirred to prepare a thermoplastic polyurethane bone repair membrane by electrospinning.
[0021] The step 1) is specifically as follows:
[0022] 1.1) Mixing the template solution and the catalyst solution, and then adding a precursor substance thereto at regular intervals, adding a different precursor substance each time, to obtain a mixed solution;
[0023] 1.2) stirring and aging the mixed solution obtained in step 1.1) to obtain a white sol;
[0024] 1.3) centrifuging the white sol obtained in step 1.2), washing it with anhydrous ethanol and deionized water, and drying it to obtain a white powder;
[0025] 1.4) The white powder obtained in step 1.3) is placed in a muffle furnace and calcined to obtain bioactive glass microspheres.
[0026] In the step 1.1), the template solution is a hexadecyltrimethylammonium bromide solution with a mass concentration of 4 to 4.6 mg / mL, the catalyst solution is an ammonia solution with a mass concentration of 25% to 28%, and the volume ratio of the template solution to the catalyst solution is (100 to 120): (1 to 2);
[0027] In the step 1.2), the stirring time is 5 to 8 hours, the aging temperature is room temperature, and the aging time is 24 to 40 hours;
[0028] In the step 1.3), the calcination temperature is 600-700° C. and the calcination time is 5-8 hours.
[0029] In the step 1.1), the precursor material is added five times at intervals of 1 to 2 hours, and the stirring period is 1 to 2 hours. The five precursor materials are respectively tetraethyl orthosilicate, triethyl phosphate, tributyl borate, calcium nitrate tetrahydrate and sodium selenite pentahydrate. The molar ratio of tetraethyl orthosilicate, triethyl phosphate, tributyl borate, calcium nitrate tetrahydrate and sodium selenite pentahydrate is (0 to 50): (2 to 2.5): (5 to 30): (30 to 36): (0 to 5).
[0030] The step 2) is specifically as follows:
[0031] 2.1) dispersing the bioactive glass microspheres prepared in step 1) into an N,N-dimethylformamide solution, adding thermoplastic polyurethane particles and stirring, and then ultrasonicating until the bioactive glass microspheres are uniformly dispersed in the solution to obtain a thermoplastic polyurethane bioactive glass solution;
[0032] 2.2) The thermoplastic polyurethane bioactive glass solution obtained in step 2.1) is electrospun to obtain a thermoplastic polyurethane bioactive glass fiber membrane, namely a thermoplastic polyurethane bone repair membrane.
[0033] In the step 2.1), the ratio of the mass percentage concentration of the bioactive glass microspheres to the mass of the thermoplastic polyurethane particles is (1-7):100;
[0034] In the step 2.2), the propulsion speed of electrospinning is 0.5-1 mL / h, the applied voltage is 10-20 kV, the receiving distance is 10-20 cm, and the diameter of the fiber formed by electrospinning is 400-4000 nm.
[0035] 3. Application of a highly active thermoplastic polyurethane bone repair membrane
[0036] Application in clinical bone tissue engineering, specifically the application of materials for artificial bone repair.
[0037] The preparation method of the present invention is simple, and the prepared bone repair membrane has excellent and adjustable biological activity, good mechanical properties, orderly and controllable degradation performance, certain antibacterial and biocompatibility, and has high porosity, can improve osteoblast activity, and has broad application prospects in the field of bone repair materials.
[0038] The invention provides a high-activity thermoplastic polyurethane bone repair membrane. The organic component adopts thermoplastic polyurethane, and the inorganic component adopts selenium-doped borosilicate-based bioactive glass. The bone repair membrane material is prepared by mixing the organic component and the inorganic component.
[0039] The present invention has the following beneficial effects:
[0040] The average particle size of the borosilicate bioactive glass nano-microspheres in the present invention is at the nanometer scale, and the prepared repair membrane material has a high specific surface area and porosity, is conducive to the adhesion and proliferation of cells, and promotes the growth of osteoblasts.
[0041] The present invention mixes thermoplastic polyurethane particles and bioactive glass microspheres for electrostatic spinning, which not only makes up for the defect that the bioactive glass is relatively brittle and cannot be spun alone, but also solves the problem of insufficient bioactivity of pure thermoplastic polyurethane, and just makes up for the shortcomings of the two materials.
[0042] In addition, the present invention incorporates the selenium-doped borosilicate bioactive glass into thermoplastic polyurethane particles for spinning, which can not only improve the hydrophobicity of the repair membrane and achieve a more favorable effect for cell growth, but also release Ca 2+ and Se 4+ Therapeutic ions further induce bone tissue repair and regeneration. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Attached Figure 1 Field emission scanning electron microscope images of the bioactive glass microspheres of Example 1 and the fiber membrane of Example 4.
[0044] Attached Figure 2 This is a comparison chart of the porosity test results of the high-activity thermoplastic polyurethane bone repair membrane in Examples 2-6 and the fiber membrane in Comparative Example 1.
[0045] Attached Figure 3 This is a comparison chart of the hydrophilicity test results of the high-activity thermoplastic polyurethane bone repair membrane in Examples 2-6 and the fiber membrane in Comparative Example 1.
[0046] Attached Figure 4 This is a comparison chart of the breaking strength test results of the high-activity thermoplastic polyurethane bone repair membrane in Examples 2-6 and the fiber membrane in Comparative Example 1.
[0047] Attached Figure 5 This is a graph comparing the degradation performance test results of the high-activity thermoplastic polyurethane bone repair membrane in Examples 2-6 and the fiber membrane in Comparative Example 1.
[0048] Attached Figure 6 This is a comparison chart of the bioactivity test results of the high-activity thermoplastic polyurethane bone repair membrane in Examples 2-6 and the fiber membrane in Comparative Example 1.
[0049] Attached Figure 7 This is a comparison chart of the antibacterial performance test results of the high-activity thermoplastic polyurethane bone repair membrane in Examples 2-6 and the fiber membrane in Comparative Example 1.
[0050] Attached Figure 8 This is a comparison chart of the biocompatibility test results of the high-activity thermoplastic polyurethane bone repair membrane in Examples 2-6 and the fiber membrane in Comparative Example 1.
[0051] Attached Fig. 9 The bioactive glass microspheres of Example 1 and the fiber membranes of Example 4 were treated with therapeutic ions Ca 2+ and Se 4+ Figure 1. Results of the release behavior test. DETAILED DESCRIPTION
[0052] The present invention is described in detail below by way of examples, but the embodiments of the present invention are not limited to these examples.
[0053] Example 1: Preparation of Selenium-doped Borosilicate-based Bioactive Glass Microspheres
[0054] Selenium-doped borosilicate-based bioactive glass microspheres were synthesized by a sol-gel-template method. The specific method is as follows: 0.5 g of hexadecyltrimethylammonium bromide was dissolved in a mixed solution of 80 mL of deionized water and 40 mL of anhydrous ethanol at room temperature; after complete dissolution, 1 mL of ammonia water was added and stirred for 30 min, and then 4.58 mL of ethyl orthosilicate, 0.25 mL of triethyl phosphate, 3.15 mL of tributyl borate, 5.02 g of calcium nitrate tetrahydrate, and 0.803 g of sodium selenite pentahydrate were added in sequence every 1 h, and stirring was continued for 5 h, followed by aging at room temperature for 24 h; the white sol obtained after the reaction was centrifuged and washed with anhydrous ethanol and deionized water in sequence, and repeated three times; finally, the dried white powder was heated to 600 °C in a muffle furnace at a heating rate of 2 °C / min and calcined for 5 h to obtain bioactive glass microspheres.
[0055] Example 2: Preparation of Thermoplastic Polyurethane / 1% Bioactive Glass Fiber Membrane
[0056] The bioactive glass microspheres prepared in Example 1 with a mass equivalent to 1% of the mass of the thermoplastic polyurethane particles were weighed and dispersed in 8 g of N,N-dimethylformamide; then 2 g of the thermoplastic polyurethane particles were added and stirred for 5 h, and then ultrasonicated for 30 min to uniformly disperse the nanospheres in the solution to obtain a thermoplastic polyurethane / 1% bioactive glass solution. The thermoplastic polyurethane / 1% bioactive glass fiber membrane was obtained by electrospinning at a propulsion speed of 0.9 mL / h, a spinning voltage of 18 kV, and a receiving distance of 15 cm.
[0057] Example 3: Preparation of thermoplastic polyurethane / 2% bioactive glass fiber membrane
[0058] The bioactive glass microspheres prepared in Example 1 with a mass of 2% of the mass of the thermoplastic polyurethane particles were weighed and dispersed in 8 g of N,N-dimethylformamide; then 2 g of thermoplastic polyurethane particles were added and stirred for 5 h, and then ultrasonicated for 30 min to uniformly disperse the nanospheres in the solution to obtain a thermoplastic polyurethane / 2% bioactive glass solution. The thermoplastic polyurethane / 2% bioactive glass fiber membrane was obtained by electrospinning at a propulsion speed of 0.75 mL / h, a spinning voltage of 18 kV, and a receiving distance of 15 cm.
[0059] Example 4: Preparation of thermoplastic polyurethane / 3% bioactive glass fiber membrane
[0060] The bioactive glass microspheres prepared in Example 1 with a mass of 3% of the mass of the thermoplastic polyurethane particles were weighed and dispersed in 8 g of N,N-dimethylformamide; then 2 g of the thermoplastic polyurethane particles were added and stirred for 5 h, and then ultrasonicated for 30 min to evenly disperse the nanospheres in the solution to obtain a thermoplastic polyurethane / 3% bioactive glass solution. The thermoplastic polyurethane / 3% bioactive glass fiber membrane was obtained by electrospinning at a propulsion speed of 0.6 mL / h, a spinning voltage of 18 kV, and a receiving distance of 15 cm.
[0061] Example 5: Preparation of Thermoplastic Polyurethane / 4% Bioactive Glass Fiber Membrane
[0062] The bioactive glass microspheres prepared in Example 1, whose mass is 4% of the mass of the thermoplastic polyurethane particles, are weighed and dispersed in 8 g of N,N-dimethylformamide; then 2 g of the thermoplastic polyurethane particles are added and stirred for 5 h, and then ultrasonicated for 30 min to uniformly disperse the nanospheres in the solution to obtain a thermoplastic polyurethane / 4% bioactive glass solution. The thermoplastic polyurethane / 4% bioactive glass fiber membrane can be obtained by electrospinning at a propulsion speed of 0.5 mL / h, a spinning voltage of 18 kV, and a receiving distance of 15 cm.
[0063] Example 6: Preparation of thermoplastic polyurethane / 5% bioactive glass fiber membrane
[0064] The bioactive glass microspheres prepared in Example 1 with a mass of 5% of the mass of the thermoplastic polyurethane particles were weighed and dispersed in 8 g of N,N-dimethylformamide; then 2 g of thermoplastic polyurethane particles were added and stirred for 5 h, and then ultrasonicated for 30 min to evenly disperse the nanospheres in the solution to obtain a thermoplastic polyurethane / 5% bioactive glass solution. The thermoplastic polyurethane / 5% bioactive glass fiber membrane was obtained by electrospinning at a propulsion speed of 0.5 mL / h, a spinning voltage of 18 kV, and a receiving distance of 15 cm.
[0065] Comparative Example 1: Preparation of thermoplastic polyurethane fiber film
[0066] 2 g of thermoplastic polyurethane particles were dissolved in 8 g of N,N-dimethylformamide and stirred at room temperature for 5 h to obtain a 20 wt% polyurethane solution. The thermoplastic polyurethane fiber membrane was obtained by electrospinning at a propulsion speed of 1.3 mL / h, a spinning voltage of 18 kV, and a receiving distance of 15 cm.
[0067] The products prepared in the above examples and comparative examples were subjected to experimental performance testing.
[0068] The bioactive glass microspheres prepared in Example 1 and the fiber membrane prepared in Example 4 were fixed on a sample stage, gold-sprayed, placed in a vacuum chamber of a field emission scanning electron microscope, and observed at a voltage of 3 kV to obtain a SEM observation image. Figure 1 As shown, the microspheres of Example 1 are dispersed more evenly and are about 200 nm in size, in a uniform spherical shape.
[0069] The porosity, hydrophilicity and breaking strength of the fiber membranes prepared in Examples 2 to 6 were tested with those in Comparative Example 1. The results are shown in Table 1. Figure 2-Figure 4 As shown. The results show that the thermoplastic polyurethane / bioactive glass fiber membrane has higher porosity and hydrophilic effect than the pure thermoplastic polyurethane fiber membrane. The high porosity of the fiber membrane can reflect the high specific surface area to a certain extent, which will be more conducive to cell adhesion and proliferation.
[0070] The fiber membranes prepared in Examples 2 to 6 were subjected to pH and weight loss tests during degradation with those of Comparative Example 1 and Example 1. The results are shown in Table 1. Figure 5 The results show that compared with bioactive glass and pure thermoplastic polyurethane fiber membranes, thermoplastic polyurethane / bioactive glass fiber membranes will have a milder microenvironment in the body and the degradation rate is controllable.
[0071] The fiber membranes prepared in Examples 2 to 6 were tested for activity with those in Comparative Example 1. The results are shown in Table 1. Figure 6 The results show that after the simulated human body fluid test, a uniform hydroxyapatite layer is formed on the fiber membrane surface of the present invention, and the biological activity is significantly better than that of the pure thermoplastic polyurethane in comparative example 1.
[0072] Figure 7 Schematic diagram of the antibacterial results of Examples 2 to 6 and Comparative Example 1.
[0073] Figure 8 It is a schematic diagram of the results of the growth and proliferation of osteoblasts on the material surface of Examples 2 to 6 and Comparative Example 1.
[0074] The fiber membrane prepared in Example 4 was treated with therapeutic ion Ca 2+ and Se 4+ Release detection, ion release behavior at different time points Fig. 9 shown.
[0075] The above tests and comparisons show that the highly active thermoplastic polyurethane bone repair membrane described in the present invention not only has excellent and adjustable biological activity, good mechanical properties, orderly and controllable degradation properties, certain antibacterial and biocompatibility, but also has high porosity, can improve the activity of osteoblasts, and has broad application prospects in the field of bone repair materials.
[0076] The above-described embodiments are merely illustrative of the present invention and are not limited to the technical solutions described in the present invention. Within the protection scope of the present invention, the specific implementation schemes may be arbitrarily modified or replaced by ordinary technicians in the field.
Claims
1. A highly active thermoplastic polyurethane bone repair membrane, characterized in that: The repair film is mainly prepared by mixing thermoplastic polyurethane as an organic component and borosilicate-based bioactive glass microspheres as selenium-doped inorganic components.
2. The highly active thermoplastic polyurethane bone repair membrane according to claim 1, characterized in that: The molecular weight of the thermoplastic polyurethane is 80,000 to 100,000, and the mass percentage concentration is 10 to 20 wt%; The diameter of the bioactive glass microspheres is 160-320 nm. The components of the bioactive glass microspheres include silicon dioxide, calcium oxide, phosphorus pentoxide, boron trioxide and selenium dioxide, and the molar ratio of the components is (0-50): (30-36): (4-5): (10-60): (0-5).
3. The highly active thermoplastic polyurethane bone repair membrane according to claim 1 or 2, characterized in that: The mass ratio of the bioactive glass microspheres to the thermoplastic polyurethane particles is (1-7):
100.
4. The method for preparing the highly active thermoplastic polyurethane bone repair membrane according to any one of claims 1 to 3, characterized in that: Methods include: 1) mixing the template solution and the catalyst solution, and then adding a precursor substance thereto at intervals, adding a different precursor substance each time, and sequentially stirring, aging, centrifuging, washing, drying and calcining to obtain bioactive glass microspheres; 2) The bioactive glass microspheres prepared in step 1) are dispersed and added into N,N-dimethylformamide solution, and then thermoplastic polyurethane particles are added and stirred to prepare a thermoplastic polyurethane bone repair membrane by electrospinning.
5. The method for preparing the highly active thermoplastic polyurethane bone repair membrane according to claim 4, characterized in that: The step 1) is specifically as follows: 1.1) Mixing the template solution and the catalyst solution, and then adding a precursor substance thereto at regular intervals, adding a different precursor substance each time, to obtain a mixed solution; 1.2) stirring and aging the mixed solution obtained in step 1.1) to obtain a white sol; 1.3) centrifuging the white sol obtained in step 1.2), washing it with anhydrous ethanol and deionized water, and drying it to obtain a white powder; 1.4) The white powder obtained in step 1.3) is placed in a muffle furnace and calcined to obtain bioactive glass microspheres.
6. The method for preparing the highly active thermoplastic polyurethane bone repair membrane according to claim 5, characterized in that: In the step 1.1), the template solution is a hexadecyltrimethylammonium bromide solution with a mass concentration of 4 to 4.6 mg / mL, the catalyst solution is an ammonia solution with a mass concentration of 25% to 28%, and the volume ratio of the template solution to the catalyst solution is (100 to 120): (1 to 2); In the step 1.2), the stirring time is 5 to 8 hours, the aging temperature is room temperature, and the aging time is 24 to 40 hours; In the step 1.3), the calcination temperature is 600-700° C. and the calcination time is 5-8 hours.
7. The method for preparing the highly active thermoplastic polyurethane bone repair membrane according to claim 5, characterized in that: In the step 1.1), the precursor material is added five times at intervals of 1 to 2 hours, and the stirring period is 1 to 2 hours. The five precursor materials are respectively tetraethyl orthosilicate, triethyl phosphate, tributyl borate, calcium nitrate tetrahydrate and sodium selenite pentahydrate. The molar ratio of tetraethyl orthosilicate, triethyl phosphate, tributyl borate, calcium nitrate tetrahydrate and sodium selenite pentahydrate is (0 to 50): (2 to 2.5): (5 to 30): (30 to 36): (0 to 5).
8. The method for preparing the highly active thermoplastic polyurethane bone repair membrane according to claim 4, characterized in that: The step 2) is specifically as follows: 2.1) dispersing the bioactive glass microspheres prepared in step 1) into an N,N-dimethylformamide solution, adding thermoplastic polyurethane particles and stirring, and then ultrasonicating until the bioactive glass microspheres are uniformly dispersed in the solution to obtain a thermoplastic polyurethane bioactive glass solution; 2.2) The thermoplastic polyurethane bioactive glass solution obtained in step 2.1) is electrospun to obtain a thermoplastic polyurethane bioactive glass fiber membrane, namely a thermoplastic polyurethane bone repair membrane.
9. The method for preparing the highly active thermoplastic polyurethane bone repair membrane according to claim 8, characterized in that: In the step 2.1), the ratio of the mass percentage concentration of the bioactive glass microspheres to the mass of the thermoplastic polyurethane particles is (1-7):100; In the step 2.2), the propulsion speed of electrospinning is 0.5-1 mL / h, the applied voltage is 10-20 kV, the receiving distance is 10-20 cm, and the diameter of the fiber formed by electrospinning is 400-4000 nm.
10. Use of the highly active thermoplastic polyurethane bone repair membrane according to any one of claims 1 to 3 or the highly active thermoplastic polyurethane bone repair membrane prepared by the preparation method according to any one of claims 4 to 9, characterized in that: Application in clinical bone tissue engineering.