Hierarchical fiber membrane material for full-layer plugging of skull base as well as preparation method and application of hierarchical fiber membrane material
A hierarchical fiber membrane material is developed through electrospinning and tape casting, addressing the structural and biodegradability issues of existing materials by providing effective sealing and support for skull base repairs, promoting healing and preventing cerebrospinal fluid leakage.
Patent Information
- Application Number
- CN202411286919.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-06
AI Technical Summary
Existing skull base repair materials lack a structure similar to dura mater + bone + mucosa, are expensive, or not biodegradable, failing to provide adequate mechanical support and sealing against cerebrospinal fluid leakage, which can lead to serious complications.
A method involving electrospinning and tape casting to create a hierarchical fiber membrane material with alternating layers of electrospun and cast membranes, using solutions of gelatin, silk fibroin, chitosan, and polyvinyl alcohol, cross-linked with glutaraldehyde and loaded with hydroxyapatite, to form a structure that mimics dura mater + bone + mucosa.
The hierarchical fiber membrane provides effective sealing and mechanical support, preventing cerebrospinal fluid leakage, promoting cell attachment and vascularization, and degrading within the body's healing cycle, with enhanced mechanical properties and biocompatibility.
Smart Images

Figure CN119075020A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of medical biomaterials, and in particular relates to a hierarchical fiber membrane material for full-thickness occlusion of skull base, and a preparation method and application thereof. Background Art
[0002] Skull base trauma is a serious physical trauma, which is critical and complicated. Among them, cerebrospinal fluid leakage is the most difficult problem in nasal skull base surgery. Because cerebrospinal fluid rhinorrhea indicates that there is a connection between the nasal cavity and the skull base, antibiotics must be used for anti-infection treatment, otherwise retrograde infection will occur and meningitis will occur. The patient will experience serious consequences such as headache, dizziness, nausea, coma, and even death.
[0003] With the improvement of skull base repair materials and the development of new materials in recent years, the clinical experience of multiple reconstruction of skull base repair after neuroendoscopy has been summarized. The reconstruction method of dura mater + bone + mucosa similar to the physiological anatomy of skull base is more in line with the physiological structure of the human body and is also conducive to the regeneration of dura mater, bone and mucosa. The development of skull base biomaterials has also been gradually replaced on this basis. Therefore, many dura mater and bone-like biomaterials have been derived clinically for multiple reconstruction of skull base repair. In terms of clinical application, many biomaterials have their own advantages and disadvantages: materials such as titanium mesh, porous polyethylene (Polyethylene, PE) and polyether ether ketone (Polyether ether ketone, PEEK), although they have high mechanical strength, cannot be absorbed by the human body, and the price in the market is also very expensive, which cannot benefit the majority of patients on a large scale; materials such as gelatin, silk fibroin and chitosan not only have certain mechanical strength, but are also degradable in the human body and can be absorbed by the human body. Compared with materials such as titanium mesh and polyether ether ketone, they are relatively cheap and easy to mass produce. Electrospinning technology can produce porous fiber membranes, and tape casting technology can produce dense films. A single material and preparation method cannot meet the complex environment of skull base trauma. It is necessary to combine multiple materials and electrospinning and tape casting to prepare skull base repair materials similar to dura mater + bone + mucosa. Summary of the invention
[0004] In view of the shortcomings of the above-mentioned prior art, the first purpose of the present invention is to provide a method for preparing a hierarchical fiber membrane material for full-thickness occlusion of the skull base, wherein the material prepared by the method has a structure similar to dura mater + bone + mucosa.
[0005] The second object of the present invention is to provide a hierarchical fiber membrane material prepared by the above method, which has the characteristics of being low in price and capable of being absorbed by the human body.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a hierarchical fiber membrane material for full-thickness occlusion of the skull base, comprising the following steps:
[0007] (1) preparing an electrospinning solution;
[0008] (2) placing the electrospinning solution into a syringe, putting on a G20 needle and placing it on a propulsion pump, setting the electrospinning parameters for spinning, and drying the membrane on the receiving plate to obtain an electrospinning membrane;
[0009] (3) immersing the electrospun membrane in a glutaraldehyde solution, then washing it; then immersing it in a functional material suspension for loading, and then drying it to obtain a fiber membrane;
[0010] (4) then repeating steps (1) to (3) to prepare a fiber membrane, and then preparing a casting liquid, and using a casting film to fill between the fiber membranes to obtain a hierarchical fiber membrane material;
[0011] The electrospinning solution is a mixed solution of gelatin and silk fibroin in glacial acetic acid; or the electrospinning solution is a mixed solution of water, tetraethyl silicate and phosphoric acid and polyvinyl alcohol solution; or the electrospinning solution is a mixed solution of chitosan in glacial acetic acid and polyvinyl alcohol aqueous solution.
[0012] As a preferred embodiment of the present invention, the mass fraction of glutaraldehyde is 25%.
[0013] As a preferred embodiment of the present invention, the mass percentage of the solute in the electrospinning solution is 5-30%, and the solute is gelatin and silk fibroin, polyvinyl alcohol or chitosan and polyvinyl alcohol.
[0014] As a preferred embodiment of the present invention, in step (2), the electrospinning parameters are: positive pressure: 12 to 20 KV, negative pressure: -3 to -8 KV, propulsion pump rate: 3 to 15 mm / h, and receiving device distance: 10 to 25 cm.
[0015] As a preferred embodiment of the present invention, the electrospinning membrane is immersed in the glutaraldehyde solution for 12 hours.
[0016] As a preferred embodiment of the present invention, the concentration of the functional material in the functional material suspension is 10 mg / ml, and the functional material is at least one of hydroxyapatite, silk fibroin, polyvinyl alcohol, and resveratrol.
[0017] As a preferred embodiment of the present invention, in the step (3), the immersion time in the functional material suspension is 6 hours.
[0018] As a preferred embodiment of the present invention, the casting liquid is an electrospinning solution or a silica sol.
[0019] As a preferred embodiment of the present invention, in the step (3), the specific parameters of the casting liquid filling are: casting device temperature: 10-60°C, casting machine height: 50rpm, scraper height: 0.1-1mm. The present invention performs casting on a casting molding composite technology device, and under the action of the casting liquid, the hierarchical fiber membrane is prepared by layer-by-layer self-assembly between the membranes.
[0020] As a preferred embodiment of the present invention, the thickness of the fiber membrane is 0.01 mm-0.5 mm, and the thickness of the layered fiber membrane material is 0.5 mm-2 mm.
[0021] The present invention also claims protection for the hierarchical fiber membrane material prepared by the method for preparing the hierarchical fiber membrane material.
[0022] The layered fiber membrane material comprises three layers of fiber membranes and two layers of cast membranes, and the fiber membranes and the cast membranes are alternately stacked.
[0023] The present invention also protects the application of the hierarchical fiber membrane material in full-thickness occlusion of the skull base.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention obtains a fiber membrane by electrospinning, and then functionalizes the fiber membrane or loads drugs on it. To facilitate drug loading and functionalization, the fiber membrane is first soaked in glutaraldehyde to facilitate subsequent drug loading and functionalization. The fiber membrane is then immersed in a specific solution for drug loading or functionalization. Finally, a cast membrane is prepared by tape casting technology, and the fiber membrane and the cast membrane are alternately superimposed to prepare a hierarchical fiber membrane scaffold with three layers of fiber membrane and two layers of cast membrane, a total of five layers. This structure has a blocking and supporting effect. The cast membrane plays a blocking role to prevent brain nasal fluid leakage or tissue fluid leakage, and the fiber membrane plays a supporting role. In the treatment of bone defects, the repair material must replace the bone defect and play a certain supporting role.
[0026] (2) The hierarchical fiber membrane material of the present invention has a large specific surface area, and the hierarchical fiber membrane structure on the surface provides favorable conditions for cell attachment and growth, the transport of nutrients, and the vascularization of surrounding tissues. In addition, the cast multilayer self-assembly enhances the mechanical properties of the hierarchical fiber membrane, thereby avoiding morphological changes caused by body stress after surgical implantation in the body, resulting in surgical failure. Finally, the hierarchical fiber membrane material of the present invention has good biocompatibility and has no obvious immune rejection reaction after implantation in the body. Moreover, its degradation performance meets the bone repair cycle, with a degradation rate of less than 20% within three months. As the bone defect heals, the degradation rate of the hierarchical fiber membrane material reaches more than 80% within six months, and the loaded functional materials and / or drug-loaded components will effectively reach the bone defect site for local targeted treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The diagrams are the electrospinning process diagram and the tape-casting composite technology diagram; (a) Schematic diagram of the electrospinning process; (b) Schematic diagram of the tape-casting composite technology.
[0028] Figure 2 This is a structural diagram of the layered fibrous membrane material for full-thickness closure of the skull base.
[0029] Figure 3 These are scanning electron microscope images of the gelatin / silk fibroin hierarchical fiber membrane material prepared in Example 1; (a) is a scanning electron microscope image of the gelatin / silk fibroin electrospun membrane; (b) is a scanning electron microscope image of the gelatin / silk fibroin cast membrane; (c) is a scanning electron microscope image of the cross-section of the gelatin / silk fibroin hierarchical fiber membrane.
[0030] Figure 4 These are scanning electron microscope images of the polyvinyl alcohol hierarchical fiber membrane material prepared in Example 2; (a) is a scanning electron microscope image of a polyvinyl alcohol electrospinning membrane; (b) is a scanning electron microscope image of a polyvinyl alcohol cast membrane; (c) is a scanning electron microscope image of a cross-section of a polyvinyl alcohol hierarchical fiber membrane.
[0031] Figure 5 These are scanning electron microscope images of the chitosan / polyvinyl alcohol hierarchical fiber membrane materials prepared in Example 3; (a) is a scanning electron microscope image of the chitosan / polyvinyl alcohol electrospun membrane; (b) is a scanning electron microscope image of the chitosan / polyvinyl alcohol cast membrane; (c) is a scanning electron microscope image of the cross section of the chitosan / polyvinyl alcohol hierarchical fiber membrane.
[0032] Figure 6 Actual picture of the gelatin / silk fibroin layered fiber membrane material prepared in Example 1 and its blocking effect on SBF (simulated body fluid - added sky blue CuSO4 solution) in vitro; (a) Actual picture of the gelatin / silk fibroin layered fiber membrane; (b) Blocking effect of the gelatin / silk fibroin layered fiber membrane on SBF (simulated body fluid) at 0 min in vitro; (c) Blocking effect of the gelatin / silk fibroin layered fiber membrane on SBF at 30 min in vitro. DETAILED DESCRIPTION
[0033] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0034] Example 1
[0035] A method for preparing a hierarchical fiber membrane material for full-thickness skull base occlusion comprises the following steps:
[0036] (1) 0.9 g of gelatin particles with a molecular weight of 300,000 to 500,000 were dissolved in glacial acetic acid (purity: 99.5%, molecular weight: 60.05), and silk fibroin (molecular weight: 100 to 152 kDa) was added after being fully stirred for 3 hours. After being fully dissolved, the mixture was subjected to ultrasonic defoaming and then allowed to stand to obtain an electrospinning solution.
[0037] (2) The electrospinning solution was placed in a syringe, and a G20 needle was put on the propulsion pump, and the electrospinning parameters were set for spinning. The membrane on the receiving plate was dried to obtain an electrospinning membrane; the electrospinning parameters were positive pressure: 20 KV, negative pressure: -5 KV, propulsion pump rate: 12 mm / hour), and a flat plate was prepared for receiving (receiving plate distance: 12 cm).
[0038] (3) The electrospun membrane was immersed in a glutaraldehyde solution (mass fraction: 25%, molecular weight: 100.12) for 12 hours to cross-link the fiber membrane and improve the mechanical properties of the fiber membrane. The fiber membrane was then washed and allowed to stand. The membrane was then immersed in a 10 mg / ml hydroxyapatite suspension for 6 hours for loading and then freeze-dried to obtain a fiber membrane.
[0039] (4) Then repeat steps (1)-(3) to prepare fiber membranes, cut the fiber membranes into regular sizes, and then prepare casting liquid (i.e., electrospinning solution), and use cast membranes to fill between the fiber membranes to prepare a two-layer cast membrane and a three-layer fiber membrane structure material; the cast membranes and the fiber membranes are alternately stacked.
[0040] (5) After drying the material obtained in step (4), it was trimmed to obtain a thickness of 0.8 mm and an area of 1*1 (cm 2 )'s hierarchical fiber membrane material.
[0041] Example 2
[0042] A method for preparing a hierarchical fiber membrane material for full-thickness skull base occlusion comprises the following steps:
[0043] (1) Dissolve 2 g of polyvinyl alcohol (molecular weight: 75,000) particles in 18 ml of pure water, heat to 80°C in a water bath and stir thoroughly to dissolve them into solution A; mix 5 ml of pure water, 5 ml of tetraethyl silicate (purity: 98% molecular weight: 208.33) and 0.2 ml of phosphoric acid (concentration: 85% molecular weight: 98.00) solution and stir for 6 hours to obtain solution B; mix solution A and solution B in a volume ratio of 5:3 and stir for 3 hours to obtain an electrospinning solution.
[0044] (2) The electrospinning solution was placed in a syringe, and a G20 needle was put on the propulsion pump. The electrospinning parameters were set for spinning, and the membrane on the receiving plate was dried to obtain an electrospinning membrane; the electrospinning parameters were positive pressure: 18KV, negative pressure: -5KV, propulsion pump rate: 9mm / hour), and a flat plate was prepared for receiving (receiving plate distance: 12cm).
[0045] (3) The electrospun membrane was immersed in a glutaraldehyde solution (mass fraction: 25%) for 12 hours to cross-link the fiber membrane and improve the mechanical properties of the fiber membrane. The fiber membrane was then washed and allowed to stand. The membrane was then immersed in a 10 mg / ml hydroxyapatite suspension for 6 hours for loading and then freeze-dried to obtain a fiber membrane.
[0046] (4) Then repeat steps (1)-(3) to prepare fiber membranes, cut the fiber membranes into regular sizes, and then prepare casting liquid (i.e., electrospinning solution), and use cast membranes to fill between the fiber membranes to prepare a two-layer cast membrane and a three-layer fiber membrane structure material; the cast membranes and the fiber membranes are alternately stacked.
[0047] (5) After drying the material obtained in step (4), it was trimmed to obtain a thickness of 0.8 mm and an area of 1*1 (cm 2 )'s hierarchical fiber membrane material.
[0048] Example 3
[0049] A method for preparing a hierarchical fiber membrane material for full-thickness skull base occlusion comprises the following steps:
[0050] (1) Dissolve 1 g of chitosan particles with a molecular weight of 80,000 in 2.5 ml of glacial acetic acid (purity: 99.5%, molecular weight: 60.05) and 7.5 ml of water, heat to 40°C in a water bath and stir for 3 hours to obtain solution C; dissolve 2 g of polyvinyl alcohol (molecular weight: 75,000) particles in 18 ml of pure water, heat to 80°C in a water bath and stir for 3 hours to fully dissolve them to obtain solution D; mix solution C and solution D in a volume ratio of 1:1, stir for 2 hours, and obtain an electrospinning solution.
[0051] (2) The electrospinning solution was placed in a syringe, and a G20 needle was put on the propulsion pump, and the electrospinning parameters were set for spinning. The membrane on the receiving plate was dried to obtain an electrospinning membrane; the electrospinning parameters were positive pressure: 25KV, negative pressure: -5KV, propulsion pump rate: 12mm / hour), and a flat plate was prepared for receiving (receiving plate distance: 25cm).
[0052] (3) The electrospun membrane was immersed in a glutaraldehyde solution (mass fraction: 25%, molecular weight: 100.12) for 12 hours to cross-link the fiber membrane and improve the mechanical properties of the fiber membrane, and then washed and allowed to stand; then immersed in a 10 mg / ml hydroxyapatite suspension for 6 hours for loading, and then freeze-dried to obtain a fiber membrane.
[0053] (4) Then repeat steps (1)-(3) to prepare fiber membranes, cut the fiber membranes into regular sizes, and then prepare casting liquid (i.e., electrospinning solution), and use cast membranes to fill between the fiber membranes to prepare a two-layer cast membrane and a three-layer fiber membrane structure material; the cast membranes and the fiber membranes are alternately stacked.
[0054] (5) After drying the material obtained in step (4), it was trimmed to obtain a thickness of 0.8 mm and an area of 1*1 (cm 2 )'s hierarchical fiber membrane material.
[0055] Comparative Example 1
[0056] For comparison, this comparative example is different from Example 3 in that the tape casting composite technology and the hierarchical fiber membrane structure in step (4) are not used, and the other steps are the same as those in Example 3, specifically:
[0057] (1) Dissolve 1 g of chitosan particles with a molecular weight of 80,000 in 2.5 ml of glacial acetic acid (purity: 99.5%, molecular weight: 60.05) and 7.5 ml of water, heat to 40°C in a water bath and stir for 3 hours to obtain solution C; dissolve 2 g of polyvinyl alcohol (molecular weight: 75,000) particles in 18 ml of pure water, heat to 80°C in a water bath and stir for 3 hours to fully dissolve them to obtain solution D; mix solution C and solution D in a volume ratio of 1:1, stir for 2 hours, and obtain an electrospinning solution.
[0058] (2) The electrospinning solution was placed in a syringe, and a G20 needle was put on the propulsion pump, and the electrospinning parameters were set for spinning. The membrane on the receiving plate was dried to obtain an electrospinning membrane; the electrospinning parameters were positive pressure: 20 KV, negative pressure: -5 KV, propulsion pump rate: 12 mm / hour), and a flat plate was prepared for receiving (receiving plate distance: 12 cm).
[0059] (3) The electrospun membrane was immersed in a glutaraldehyde solution (mass fraction: 25%, molecular weight: 100.12) for 12 hours to cross-link the fiber membrane and improve the mechanical properties of the fiber membrane. The fiber membrane was then washed and allowed to stand. The membrane was then immersed in a 10 mg / ml hydroxyapatite suspension for 6 hours for loading and then freeze-dried to obtain a fiber membrane.
[0060] (4) After drying the fiber membrane obtained in step (3), trimming is performed to obtain a fiber membrane with a thickness of 0.1 mm and an area of 1*1 (cm2 ) fiber membrane material.
[0061] The contact angle and tensile strength of the products prepared in Examples 1 to 3 and Comparative Example 1 were tested and compared. The test results are shown in Table 1.
[0062] Table 1
[0063] Test items Contact angle Tensile strength(MPa) Example 1 62.5° 3.31±0.08 Example 2 65.1° 5.66±0.28 Example 3 67.1° 5.83±0.11 Comparative Example 1 105.49° 3.39±0.31
[0064] Compared with comparative example 1, the tensile strength of Examples 1 to 3 is increased, and the hierarchical fiber membrane has better mechanical properties than the electrospun membrane. The contact angle of Example 3 is smaller than that of Comparative Example 1 (the smaller the contact angle, the better the hydrophilicity), indicating that the hierarchical fiber membrane is more hydrophilic than the electrospun membrane and is more conducive to cell adhesion. After cross-linking with glutaraldehyde, immersion in a hydroxyapatite suspension for loading, and freeze-drying, layer-by-layer self-assembly is performed using a tape casting technique, which can be well applied in clinical surgical treatment of full-thickness occlusion of the skull base. Due to the complex intracranial environment and skull base trauma and defect symptoms caused by various reasons, on the one hand, materials are needed to block intracranial cerebrospinal fluid leakage to prevent cerebrospinal fluid from leaking into the cerebral cortex, causing more serious complications of infection and secondary surgical injuries; on the other hand, the intracranial bone must have a certain mechanical strength to adapt to the intracranial pressure environment.
[0065] The single-layer electrospun membrane prepared in comparative example 1 was not self-assembled layer by layer by tape casting technology, and the physiological structure of non-dura mater + bone + mucosa could not replace the damaged skull tissue to provide a certain support, and its own tensile strength and hydrophilicity did not meet the needs of skull base repair. The blocking of cerebrospinal fluid leakage requires that the repair material has a certain support and sealing effect at the same time. Failure to block cerebrospinal fluid leakage will cause more serious inflammation and complications.
[0066] Figure 6 As shown in the figure, the SBF solution did not decrease significantly after 30 minutes, indicating that the gelatin / silk fibroin hierarchical fiber membrane has a certain blocking effect on the SBF solution in vitro. The gelatin / silk fibroin hierarchical fiber membrane has a blocking effect on the SBF solution in vitro, mainly because the gelatin / silk fibroin cast membrane (such as Figure 3 (b) The surface structure is dense and there is basically no pore, so it can block the SBF solution. Examples 1-3 can achieve the blocking effect, while Comparative Example 1 has no blocking effect.
[0067] The present invention adds the hydroxyapatite of step (3) of Example 1 to the electrospinning solution for electrospinning membrane preparation, and the finally obtained hierarchical fiber membrane material has an increased contact angle and a reduced tensile strength compared to Example 1. In addition, the present invention modifies the electrospinning membrane with glutaraldehyde, which can overcome the problem of increased contact angle and reduced tensile strength caused by directly adding the electrospinning solution to prepare the electrospinning membrane. Moreover, the present invention uses glutaraldehyde to modify the electrospinning membrane, which can enhance hydrophilicity and substantially keep the tensile strength from decreasing compared to polydopamine modification.
[0068] The present invention uses a casting liquid between two layers of electrospinning membranes to prepare a cast membrane. Compared with the existing preparation method of directly performing electrospinning on the cast membrane, the cast membrane has higher tensile strength, and the cast membrane is more tightly combined with the electrospinning membrane, and has stronger blocking effect and supporting effect.
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a hierarchical fiber membrane material for full-thickness occlusion of skull base, characterized in that: The steps include: (1) preparing an electrospinning solution; (2) placing the electrospinning solution into a syringe, putting on a G20 needle and placing it on a propulsion pump, setting the electrospinning parameters for spinning, and drying the membrane on the receiving plate to obtain an electrospinning membrane; (3) immersing the electrospun membrane in a glutaraldehyde solution, then washing it; then immersing it in a functional material suspension for loading, and then drying it to obtain a fiber membrane; (4) Repeating steps (1) to (3) to prepare a fiber membrane, and then preparing a casting liquid, and using a casting film to fill between the fiber membranes to obtain a hierarchical fiber membrane material; The electrospinning solution is one of the following solutions: a glacial acetic acid solution of gelatin and silk fibroin; a mixed solution of a mixed solution of water, tetraethyl silicate and phosphoric acid and a polyvinyl alcohol solution; a mixed solution of a glacial acetic acid solution of chitosan and a polyvinyl alcohol aqueous solution.
2. The method for preparing the hierarchical fiber membrane material for full-thickness skull base occlusion according to claim 1, characterized in that: The mass fraction of the glutaraldehyde solution is 25%.
3. The method for preparing the hierarchical fiber membrane material for full-thickness skull base occlusion according to claim 1, characterized in that: The mass percentage of the solute in the electrostatic spinning solution is 5-30%, and the solute is gelatin and silk fibroin, polyvinyl alcohol or chitosan and polyvinyl alcohol.
4. The method for preparing the hierarchical fiber membrane material for full-thickness skull base occlusion according to claim 1, characterized in that: In the step (2), the electrospinning parameters are: positive pressure: 12 to 20 KV, negative pressure: -3 to -8 KV, propulsion pump rate: 3 to 15 mm / h, receiving device distance: 10 to 25 cm, and spinning time until the spinning solution is exhausted.
5. The method for preparing the hierarchical fiber membrane material for full-thickness skull base occlusion according to claim 1, characterized in that: In the step (3), the electrospun membrane is immersed in the glutaraldehyde solution for 12 hours; The immersion time in the functional material suspension was 6 hours.
6. The method for preparing the hierarchical fiber membrane material for full-thickness occlusion of skull base according to claim 1, characterized in that: The concentration of the functional material in the functional material suspension is 10 mg / ml, and the functional material is at least one of hydroxyapatite, silk fibroin, polyvinyl alcohol, and resveratrol.
7. The method for preparing the hierarchical fiber membrane material for full-thickness occlusion of skull base according to claim 1, characterized in that: In the step (3), the specific parameters of the casting liquid filling are: casting device temperature: 10-60°C, casting machine rotation speed: 50rpm, scraper height: 0.1-1mm; the casting liquid is an electrospinning solution or silica sol.
8. The hierarchical fiber membrane material prepared by the method for preparing a hierarchical fiber membrane material for full-thickness occlusion of skull base according to any one of claims 1 to 7.
9. The layered fiber membrane material according to claim 8, characterized in that: The hierarchical fiber membrane material comprises three layers of electrospun membranes and two layers of cast membranes, and the electrospun membranes and the cast membranes are alternately stacked; the thickness of the electrospun membranes is 0.01-0.5 mm, and the thickness of the hierarchical fiber membrane material is 0.5-2 mm.
10. Use of the layered fiber membrane material as claimed in claim 8 or 9 for full-thickness occlusion of the skull base.