Preparation method of hollow fiber membrane with catalytic performance

By optimizing the raw material ratio and preparation process, and using spinneret technology to prepare hollow fiber membranes, the problems of uneven catalytic performance and insufficient stability are solved, and efficient and low-cost catalyst applications are achieved, which are suitable for industrial-scale production.

CN119075701APending Publication Date: 2024-12-06ZHEJIANG NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411183020.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing hollow fiber membranes have problems such as uneven distribution, insufficient stability, complex preparation process and high cost in terms of catalytic performance, which is difficult to meet the needs of industrial-scale applications.

Method used

By optimizing the raw material ratio and preparation process, using the reasonable ratio of polymer matrix materials, catalyst active components, plasticizers, stabilizers and solvents, the hollow fiber membrane is prepared by spinning technology to control the pore size and wall thickness, and improve catalysis Uniformity and stability of active components.

Benefits of technology

It significantly improves the catalytic efficiency and selectivity, reduces the catalyst usage and production cost, realizes the stability of the hollow fiber membrane under high temperature and strong acid-base conditions, is suitable for large-scale production, and improves mechanical strength and reaction rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of hollow fiber membranes, in particular to a preparation method of a hollow fiber membrane with catalytic performance. The raw materials comprise a polymer matrix material, a catalyst active component, a plasticizer, a stabilizer composition, a dispersant and a solvent. The preparation method comprises the following steps: mixing the weighed raw materials to form a uniform mixed solution; extruding the mixed solution through a spinning nozzle of hollow fiber membrane preparation equipment, and arranging a coagulating bath outside the spinning nozzle, so that fibers are cured in the coagulating bath to form a hollow fiber membrane; washing the cured hollow fiber membrane, and removing the residual solvent and plasticizer on the surface; and drying the washed hollow fiber membrane to obtain the hollow fiber membrane with catalytic performance. By optimizing the raw material ratio and the preparation process, the hollow fiber membrane with excellent catalytic performance, good stability and low cost can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hollow fiber membrane preparation, and in particular to a method for preparing a hollow fiber membrane with catalytic performance. Background Art

[0002] In modern industrial production, the use of catalysts plays a vital role in improving the efficiency and selectivity of chemical reactions. Traditional catalysts are mostly in powder or granular form, which have some inherent defects during use, such as difficulty in separation, easy loss, and easy deactivation of active components. In order to overcome these problems, researchers have developed a variety of new catalyst carriers, among which hollow fiber membranes have attracted widespread attention due to their unique structure and performance.

[0003] Hollow fiber membrane is a fiber material with a hollow structure, with a cavity inside and a dense or porous wall outside. This structure enables the hollow fiber membrane to provide a large specific surface area to increase the loading amount of active components when used as a catalyst carrier, and to achieve rapid transmission of reactants and products through its internal cavity, thereby improving catalytic efficiency. In addition, the hollow fiber membrane has high mechanical strength and is easy to separate and recycle, which is conducive to the reuse of catalysts.

[0004] However, existing hollow fiber membranes still have certain limitations in terms of catalytic performance. For example, the catalytic active components of some hollow fiber membranes are unevenly distributed, resulting in low catalytic efficiency; some hollow fiber membranes are not stable enough in actual applications and are easily deactivated at high temperatures or under strong acid and alkali conditions; and some hollow fiber membranes are difficult to apply on a large scale due to their complex preparation process and high cost. Summary of the invention

[0005] The present invention provides a method for preparing a hollow fiber membrane with catalytic performance. By optimizing the raw material ratio and the preparation process, a hollow fiber membrane with excellent catalytic performance, good stability and low cost can be prepared.

[0006] The technical solution adopted by the present invention is: a hollow fiber membrane with catalytic performance, whose raw materials include by weight: 50-80 parts of polymer matrix material, 10-20 parts of catalyst active components, 5-15 parts of plasticizer, 1-5 parts of stabilizer composition, 1-3 parts of dispersant, and 10-30 parts of solvent.

[0007] As a further improvement of the present invention, the polymer matrix material is one or more of polyethersulfone (PES), polyetheretherketone (PEEK), and polyvinylidene fluoride (PVDF).

[0008] As a further improvement of the present invention, the catalyst active components are one or more of transition metal oxides, noble metal nanoparticles, and metal organic frameworks. Specifically, the transition metal oxides include iron oxide, manganese oxide, and copper oxide; the noble metal nanoparticles include platinum, palladium, and rhodium; and the metal organic framework includes organic framework materials based on zinc, copper, and titanium metals.

[0009] As a further improvement of the present invention, the plasticizer is one or more of phthalates, phosphates, and polyethylene glycols.

[0010] As a further improvement of the present invention, the stabilizer composition is composed of an antioxidant, a heat stabilizer, and an ultraviolet absorber, and the weight ratio of the antioxidant, the heat stabilizer, and the ultraviolet absorber is 1:1:1. Specifically, the antioxidant includes phenols, amines, and thioether compounds; the heat stabilizer includes organic phosphorus compounds and organic tin compounds; and the ultraviolet absorber includes benzotriazoles and salicylate compounds.

[0011] As a further improvement of the present invention, the dispersant is one or more of anionic surfactants and nonionic surfactants. Specifically, the anionic surfactants include alkylbenzene sulfonates and alkyl sulfates, and the nonionic surfactants include polyoxyethylene and alkylphenol polyoxyethylene ether compounds.

[0012] As a further improvement of the present invention, the solvent is one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and dimethyl sulfoxide (DMSO).

[0013] A method for preparing a hollow fiber membrane with catalytic performance comprises the following steps:

[0014] Step 1: Mix the weighed polymer matrix material, catalyst active component, plasticizer, stabilizer composition, dispersant and solvent to form a uniform mixed solution;

[0015] Step 2: extruding the mixed solution through a spinneret of a hollow fiber membrane preparation device, and setting a coagulation bath outside the spinneret, which contains a liquid that is compatible with the solvent but incompatible with the polymer matrix material, so that the fiber solidifies in the coagulation bath to form a hollow fiber membrane;

[0016] Step 3: Washing the solidified hollow fiber membrane to remove the residual solvent and plasticizer on the surface;

[0017] Step 4: Drying the washed hollow fiber membrane to obtain a hollow fiber membrane with catalytic performance.

[0018] As a further improvement of the present invention, the pore size of the hollow fiber membrane is 0.1-10 microns, and the wall thickness is 20-200 microns.

[0019] As a further improvement of the present invention, in the step 2, the liquid of the coagulation bath is one of water, ethanol, and isopropanol, and the temperature of the coagulation bath is controlled between 10-40°C; in the step 3, the washing liquid is deionized water and is washed multiple times; in the step 4, the drying treatment is carried out in a hot air circulation drying oven, and the drying temperature is controlled between 40-80°C.

[0020] Beneficial effects of the present invention: (1) By optimizing the raw material ratio and the preparation process, the hollow fiber membrane prepared by the present invention has excellent catalytic performance and can significantly improve the efficiency and selectivity of chemical reactions; since the active components are evenly distributed, the catalytic efficiency is significantly improved, thereby reducing the amount of catalyst used and reducing production costs.

[0021] (2) The hollow fiber membrane prepared by the present invention has good stability and can maintain catalytic activity under high temperature or strong acid and alkali conditions, thereby extending the service life of the catalyst; this makes it possible to reuse the catalyst in industrial production, thereby reducing production costs and environmental impact.

[0022] (3) The preparation method adopted by the present invention is simple and easy, has low cost, and is suitable for large-scale production; by selecting a suitable solvent and coagulation bath, the pore size and wall thickness of the hollow fiber membrane can be effectively controlled to meet the needs of different industrial applications.

[0023] (4) Since the hollow fiber membrane has a large specific surface area and a fast reactant transport capability, the hollow fiber membrane prepared by the present invention exhibits a higher reaction rate and conversion rate in the catalytic reaction; in addition, the hollow fiber membrane has a high mechanical strength and is easy to separate and recycle, which is conducive to the reuse of the catalyst, thereby further reducing the cost and energy consumption of industrial production. DETAILED DESCRIPTION

[0024] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0025] The invention provides a hollow fiber membrane with catalytic performance. The raw materials thereof include, by weight: 50-80 parts of polymer matrix material, 10-20 parts of catalyst active components, 5-15 parts of plasticizer, 1-5 parts of stabilizer composition, 1-3 parts of dispersant and 10-30 parts of solvent.

[0026] The polymer matrix material in the present invention is one or more of polyethersulfone (PES), polyetheretherketone (PEEK), and polyvinylidene fluoride (PVDF).

[0027] The active components of the catalyst in the present invention are one or more of transition metal oxides, noble metal nanoparticles, and metal organic frameworks. Specifically, the transition metal oxides include iron oxide, manganese oxide, and copper oxide; the noble metal nanoparticles include platinum, palladium, and rhodium; and the metal organic framework includes organic framework materials based on zinc, copper, and titanium metals.

[0028] The plasticizer in the present invention is one or more of phthalates, phosphates and polyethylene glycols.

[0029] The stabilizer composition of the present invention is composed of an antioxidant, a heat stabilizer, and an ultraviolet absorber, and the weight ratio of the antioxidant, the heat stabilizer, and the ultraviolet absorber is 1:1:1. Specifically, the antioxidant includes phenols, amines, and thioether compounds; the heat stabilizer includes organic phosphorus compounds and organic tin compounds; and the ultraviolet absorber includes benzotriazoles and salicylate compounds.

[0030] The dispersant in the present invention is one or more of anionic surfactants and nonionic surfactants. Specifically, the anionic surfactants include alkylbenzene sulfonates and alkyl sulfates, and the nonionic surfactants include polyoxyethylene and alkylphenol polyoxyethylene ether compounds.

[0031] The solvent in the present invention is one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc) and dimethyl sulfoxide (DMSO).

[0032] A method for preparing a hollow fiber membrane with catalytic performance comprises the following steps:

[0033] Step 1: Mix the weighed polymer matrix material, catalyst active component, plasticizer, stabilizer composition, dispersant and solvent to form a uniform mixed solution;

[0034] Step 2: extruding the mixed solution through a spinneret of a hollow fiber membrane preparation device, and setting a coagulation bath outside the spinneret, which contains a liquid that is compatible with the solvent but incompatible with the polymer matrix material, so that the fiber solidifies in the coagulation bath to form a hollow fiber membrane;

[0035] Step 3: Washing the solidified hollow fiber membrane to remove the residual solvent and plasticizer on the surface;

[0036] Step 4: Drying the washed hollow fiber membrane to obtain a hollow fiber membrane with catalytic performance.

[0037] The pore size of the hollow fiber membrane in the present invention is 0.1-10 microns, and the wall thickness is 20-200 microns.

[0038] In step 2 of the present invention, the liquid of the coagulation bath is one of water, ethanol and isopropanol, and the temperature of the coagulation bath is controlled between 10-40°C; in step 3, the washing liquid is deionized water and the washing is performed multiple times; in step 4, the drying treatment is performed in a hot air circulation drying oven, and the drying temperature is controlled between 40-80°C.

[0039] Embodiment 1:

[0040] This embodiment provides a method for preparing a hollow fiber membrane with catalytic performance, and the specific steps are as follows.

[0041] (i) 60 parts of polyethersulfone (PES), 15 parts of iron oxide, 10 parts of dibutyl phthalate (DBP) plasticizer, 3 parts of stabilizer composition (including 1 part each of antioxidant, heat stabilizer and ultraviolet absorber), 2 parts of anionic surfactant (alkylbenzene sulfonate) and 20 parts of N,N-dimethylformamide (DMF) solvent are mixed to form a uniform mixed solution.

[0042] (ii) The mixed solution is extruded through a spinneret of a hollow fiber membrane preparation device, and a coagulation bath is set outside the spinneret, wherein the coagulation bath contains water as a coagulation medium, and the temperature of the coagulation bath is controlled at 25° C. The fiber is solidified in the coagulation bath to form a hollow fiber membrane.

[0043] (iii) washing the solidified hollow fiber membrane with deionized water for multiple times to remove the residual solvent and plasticizer on the surface.

[0044] (iv) subjecting the washed hollow fiber membrane to hot air circulation drying treatment, with the drying temperature controlled at 60° C., to obtain a hollow fiber membrane with catalytic performance.

[0045] Embodiment 2:

[0046] This embodiment provides a method for preparing a hollow fiber membrane with catalytic performance, and the specific steps are as follows.

[0047] (i) 70 parts of polyetheretherketone (PEEK), 10 parts of platinum nanoparticles, 15 parts of tributyl phosphate (TBP) plasticizer, 5 parts of a stabilizer composition (including 1 part each of an antioxidant, a heat stabilizer, and an ultraviolet absorber), 1 part of a nonionic surfactant (polyoxyethylene compound), and 30 parts of N,N-dimethylacetamide (DMAc) solvent were mixed to form a uniform mixed solution.

[0048] (ii) The mixed solution is extruded through a spinneret of a hollow fiber membrane preparation device, and a coagulation bath is set outside the spinneret, wherein ethanol is used as a coagulation medium, and the temperature of the coagulation bath is controlled at 30° C. The fiber is solidified in the coagulation bath to form a hollow fiber membrane.

[0049] (iii) washing the solidified hollow fiber membrane with deionized water for multiple times to remove the residual solvent and plasticizer on the surface.

[0050] (iv) subjecting the washed hollow fiber membrane to hot air circulation drying treatment, with the drying temperature controlled at 50° C., to obtain a hollow fiber membrane with catalytic performance.

[0051] Embodiment 3:

[0052] This embodiment provides a method for preparing a hollow fiber membrane with catalytic performance, and the specific steps are as follows.

[0053] (i) 60 parts of polyvinylidene fluoride (PVDF), 20 parts of zinc-based metal organic framework materials, 5 parts of polyethylene glycol (PEG) plasticizer, 1.5 parts of a stabilizer composition (comprising 0.5 parts each of an antioxidant, a heat stabilizer, and an ultraviolet absorber), 3 parts of a dispersant (comprising 1.5 parts each of an anionic surfactant alkylbenzene sulfonate and a nonionic surfactant alkylphenol polyoxyethylene ether compound), and 15 parts of a dimethyl sulfoxide (DMSO) solvent are mixed to form a uniform mixed solution.

[0054] (ii) The mixed solution is extruded through a spinneret of a hollow fiber membrane preparation device, and a coagulation bath is set outside the spinneret, wherein isopropanol is used as a coagulation medium, and the temperature of the coagulation bath is controlled at 15° C. The fiber is solidified in the coagulation bath to form a hollow fiber membrane.

[0055] (iii) washing the solidified hollow fiber membrane with deionized water for multiple times to remove the residual solvent and plasticizer on the surface.

[0056] (iv) subjecting the washed hollow fiber membrane to hot air circulation drying treatment, with the drying temperature controlled at 70° C., to obtain a hollow fiber membrane with catalytic performance.

[0057] Performance Testing

[0058] In order to verify the performance of the hollow fiber membrane with catalytic performance prepared by the present invention, the following tests were performed:

[0059] (I) Porosity test:

[0060] The porosity of the hollow fiber membrane was measured by mercury intrusion porosimetry. The results showed that the porosity of the hollow fiber membranes prepared in Examples 1-3 was 75%, 70%, and 65%, respectively, indicating that the hollow fiber membrane had a high porosity, which was conducive to the catalytic reaction.

[0061] (II) Mechanical strength test:

[0062] The mechanical strength of the hollow fiber membrane was evaluated by tensile testing. The test results showed that the tensile strengths of the hollow fiber membranes prepared in Examples 1-3 were 15 MPa, 20 MPa, and 18 MPa, respectively, indicating that the hollow fiber membranes had good mechanical properties and could meet the strength requirements in practical applications.

[0063] (III) Catalytic performance test:

[0064] A specific organic reaction (hydroxylation of phenol) was used to evaluate the catalytic performance of the hollow fiber membrane. The test results showed that the hollow fiber membranes prepared in Examples 1-3 exhibited excellent activity and selectivity in the catalytic reaction, with reaction conversion rates reaching 85%, 90%, and 88%, respectively, and product selectivity exceeding 95%.

[0065] (IV) Durability test:

[0066] The hollow fiber membranes were subjected to continuous use tests to evaluate their durability. After 100 hours of continuous operation, the catalytic performance of the hollow fiber membranes prepared in Examples 1-3 decreased by no more than 5%, indicating that the hollow fiber membranes had good durability and stability.

[0067] In summary, the hollow fiber membranes with catalytic performance prepared by the present invention show excellent performance in porosity, mechanical strength, catalytic performance and durability. These hollow fiber membranes have broad application prospects in the fields of industrial catalysis, environmental protection and energy conversion.

[0068] Therefore, the method for preparing a hollow fiber membrane with catalytic properties of the present invention not only simplifies the process flow and reduces production costs, but also the prepared hollow fiber membrane has significant advantages in performance, providing efficient, stable and economical solutions for fields such as catalysis, environmental protection and energy conversion.

[0069] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A hollow fiber membrane with catalytic properties, characterized in that: The raw materials include, by weight: 50-80 parts of polymer matrix material, 10-20 parts of catalyst active components, 5-15 parts of plasticizer, 1-5 parts of stabilizer composition, 1-3 parts of dispersant and 10-30 parts of solvent.

2. The hollow fiber membrane with catalytic performance according to claim 1, characterized in that: The polymer matrix material is one or more of polyethersulfone (PES), polyetheretherketone (PEEK), and polyvinylidene fluoride (PVDF).

3. The hollow fiber membrane with catalytic performance according to claim 1, characterized in that: The catalyst active components are one or more of transition metal oxides, noble metal nanoparticles, and metal organic frameworks. Specifically, the transition metal oxides include iron oxide, manganese oxide, and copper oxide; the noble metal nanoparticles include platinum, palladium, and rhodium; and the metal organic framework includes organic framework materials based on zinc, copper, and titanium metals.

4. The hollow fiber membrane with catalytic performance according to claim 1, characterized in that: The plasticizer is one or more of phthalates, phosphates, and polyethylene glycols.

5. The hollow fiber membrane with catalytic performance according to claim 1, characterized in that: The stabilizer composition is composed of an antioxidant, a heat stabilizer, and an ultraviolet absorber, and the weight ratio of the antioxidant, the heat stabilizer, and the ultraviolet absorber is 1:1:

1. Specifically, the antioxidant includes phenols, amines, and thioether compounds; the heat stabilizer includes organic phosphorus compounds and organic tin compounds; and the ultraviolet absorber includes benzotriazoles and salicylate compounds.

6. The hollow fiber membrane with catalytic performance according to claim 1, characterized in that: The dispersant is one or more of anionic surfactants and nonionic surfactants. Specifically, the anionic surfactants include alkylbenzene sulfonates and alkyl sulfates, and the nonionic surfactants include polyoxyethylene and alkylphenol polyoxyethylene ether compounds.

7. The hollow fiber membrane with catalytic performance according to claim 1, characterized in that: The solvent is one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and dimethyl sulfoxide (DMSO).

8. A method for preparing a hollow fiber membrane having catalytic performance, characterized in that: The following steps are involved: Step 1: Mix the weighed polymer matrix material, catalyst active component, plasticizer, stabilizer composition, dispersant and solvent to form a uniform mixed solution; Step 2: extruding the mixed solution through a spinneret of a hollow fiber membrane preparation device, and setting a coagulation bath outside the spinneret, which contains a liquid that is compatible with the solvent but incompatible with the polymer matrix material, so that the fiber solidifies in the coagulation bath to form a hollow fiber membrane; Step 3: Washing the solidified hollow fiber membrane to remove the residual solvent and plasticizer on the surface; Step 4: Drying the washed hollow fiber membrane to obtain a hollow fiber membrane with catalytic performance.

9. The method for preparing a hollow fiber membrane with catalytic performance according to claim 8, characterized in that: The pore size of the hollow fiber membrane is 0.1-10 microns, and the wall thickness is 20-200 microns.

10. The method for preparing a hollow fiber membrane with catalytic performance according to claim 8, characterized in that: In the step 2, the liquid of the coagulation bath is one of water, ethanol and isopropanol, and the temperature of the coagulation bath is controlled between 10-40°C; in the step 3, the washing liquid is deionized water and the washing is performed multiple times; in the step 4, the drying treatment is performed in a hot air circulation drying oven, and the drying temperature is controlled between 40-80°C.