Controllable hierarchical pore solid amine adsorbent based on fly ash base, preparation method of adsorbent and application of adsorbent in CO2 trapping

Through the combination of fly ash-based multi-stage porous SiO2 carrier and organic amine, the problem of solid amine adsorbents being easily blocked during CO2 adsorption is solved, and efficient and low-cost CO2 capture is achieved, suitable for industrial applications and waste is achieved High-value utilization of matter.

CN119075924APending Publication Date: 2024-12-06HENAN UNIVERSITY

Patent Information

Application Number
CN202411574162.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing solid amine adsorbents are prone to blocking the pores during CO2 adsorption, increasing the CO2 mass transfer resistance. In addition, industrial applications are subject to high costs and low efficiency, making it difficult to achieve large-scale negative carbon emission targets.

Method used

Using fly ash as raw material, silicon-rich precursor liquid is obtained through alkali-soluble leaching, combined with gas-phase-assisted precipitation technology and spaced self-assembly method to synthesize multi-stage porous SiO2 carriers, and functionalized with organic amine impregnation to prepare low-cost and high-performance multi-stage porous solid amine adsorbent.

Benefits of technology

It reduces the mass transfer resistance during CO2 adsorption process, improves the adsorption capacity, realizes the high-value utilization of waste, significantly reduces the preparation cost of adsorbent, is suitable for industrial applications, and has good cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a method for preparing a hierarchical pore SiO2-based solid amine adsorbent by extracting Si element from fly ash and application of the hierarchical pore SiO2-based solid amine adsorbent to capture CO2 in flue gas. The preparation method of the adsorbent comprises the following steps: (1) calcining fly ash, and carrying out alkali dissolution extraction to obtain a silicon-rich solution; (2) analyzing the concentration of the silicon solution, and selecting a proper template agent to synthesize a silicon oxide precursor through a gas-phase-assisted precipitation technology; (3) on the basis of the step (2), changing the secondary adding interval time and adding amount of the silicon solution through an interval self-assembly method to realize controllable regulation and control of the hierarchical pore structure; calcining in an air atmosphere to obtain a hierarchical pore SiO2 carrier; and uniformly dispersing in an organic amine dispersion liquid, and drying by distillation to obtain a solid substance, namely the hierarchical pore solid amine adsorbent. The adsorbent obtained by the invention has rich pore structures, can reduce the mass transfer resistance in the CO2 adsorption process, improves the adsorption capacity, and realizes high-value utilization of wastes at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nano material synthesis and gas adsorption, and specifically relates to a fly ash-based controllable multi-level porous solid amine adsorbent, a preparation method thereof, and an application thereof in capturing CO2. Background Art

[0002] With the acceleration of industrialization, the extensive use of fossil fuels has led to an increase in the CO2 content in the atmosphere, triggering the greenhouse effect and causing a series of global climate problems such as frequent extreme weather. Among them, carbon capture and utilization technology (CCUS) is considered to be an effective measure to achieve negative carbon emissions.

[0003] At present, the industry uses liquid amine absorption as the mainstream technology for CO2 capture, using amines to undergo a reversible and exothermic chemical reaction with CO2 to achieve the purpose of absorbing and analyzing it. However, in actual production, this technology has problems such as easy corrosion, easy volatility, high energy consumption and low toxicity, which seriously restricts its potential for large-scale development in the future. Solid amine adsorbents synthesized by impregnation or grafting of porous carriers and organic amine solvents will greatly solve the above problems. At the same time, due to its advantages such as fast adsorption rate, low reaction temperature and high stability, it has become the most promising new adsorbent. However, traditional solid amine adsorbents are prone to block the pores during the organic amine modification process, increasing the mass transfer resistance of CO2 diffusion in the pores and reducing the accessibility of CO2 to the active sites of amine adsorption. Therefore, the rational design of the pore structure to improve the dispersion of organic amines in the pores and balance the matching of surface modification and structural modification are the current breakthrough points of new solid amine adsorbents.

[0004] At present, my country's carbon emissions mainly come from coal-fired power plants, construction, industrial production, transportation and agriculture. Data show that the annual CO2 emissions from coal-fired power plants have reached billions of tons, and the capture of CO2 from this large emission point source is imminent. In addition, in addition to greenhouse gas emissions, the irrational disposal of fly ash, a secondary solid waste in this industry, will greatly become an environmental safety hazard. However, the Si / Al elements rich in the solid waste are excellent materials for preparing stable, cheap and modifiable carriers. By extracting fly ash elements and introducing templates to construct a multi-level porous structure carrier with rich pores for amino functionalization, the dispersion of organic amines and the reduction of CO2 mass transfer resistance will be promoted. Therefore, the purpose of the present invention is to develop a solid waste-based multi-level porous solid amine adsorbent for use in coal-fired power plant flue gas capture, so as to achieve high-value utilization of waste and the completion of carbon reduction and emission reduction goals. Summary of the invention

[0005] Based on the deficiencies of the prior art and aimed at the current limitations of high-value utilization of fly ash from power plant flue gas and solid amines in the field of CO2 adsorption, the present invention provides a low-cost, high-performance fly ash-based controllable multi-level porous solid amine adsorbent. The fly ash is used as raw material, and a silicon-rich precursor liquid is obtained by alkaline dissolution and leaching. A multi-level porous SiO2 carrier is synthesized by gas-assisted precipitation technology and interval self-assembly method, and is obtained by functionalization through organic amine impregnation, and has a good CO2 capture effect.

[0006] The present invention also provides a preparation method of the fly ash-based controllable multi-level porous solid amine adsorbent and its application in capturing CO2.

[0007] To achieve the above object, the present invention adopts the following technical solutions: A method for preparing a fly ash-based controllable multi-level porous solid amine adsorbent, which is composed of a multi-level porous carrier and an amine-based active component. The fly ash is used as a raw material, and after being dissolved and filtered with a sodium hydroxide solution, a multi-level porous SiO2 carrier is synthesized by a CO2 gas-assisted precipitation technology and an interval self-assembly method under the action of a template agent as a silicon source, and then the multi-level porous SiO2 carrier is impregnated in an alcohol solution of an organic amine and the solvent is evaporated to obtain a solid amine adsorbent; the method specifically comprises the following steps: (1) Mix fly ash that has been calcined at high temperature (to remove organic matter and carbon deposits) with a certain amount of NaOH and water, and then heat and stir at 110±20℃ for 0.5-3 hours. After the reaction is completed, filter while hot. The filtrate is sodium silicate solution, and the filter residue is desiliconized ash; (2) adding the sodium silicate solution and template obtained in step (1) into water, heating and stirring, and after reaching a reaction temperature of 50-90°C, introducing a certain flow rate of CO2 (CO2 / N2: 20 / 80 vol.%) gas to react for 1-5 h to obtain a precursor, and filtering, drying, and calcining to obtain a uniform mesoporous SiO2 carrier after the reaction is completed; Alternatively, during the process of introducing CO2 gas to react for 1-5 hours, a certain amount of the sodium silicate solution obtained in step (1) is added twice at a certain interval, and after the reaction is completed, the solution is filtered, dried, and calcined to obtain multi-level porous SiO2 regulated at different time intervals or different addition amounts; (3) A certain amount of organic amine is dissolved in a dispersant, and then the above-mentioned mesoporous SiO2 carrier or multi-level porous SiO2 is added and dispersed evenly. After the dispersant evaporates, it is placed in a vacuum drying oven and dried to obtain a multi-level porous solid amine adsorbent.

[0008] Specifically, in step (1), the high temperature calcination temperature can be 600-800°C, and the high temperature calcination time can be 2-4 h; the mass ratio of fly ash to NaOH is 2-4:1, such as 2:1, 3:1, 4:1, etc. Preferably, the concentration of NaOH after mixing is 15-35wt.%, such as any one of 15 wt.%, 25 wt.%, 35wt.%, etc. Further, in step (1), the stirring speed is 300-1200 rpm, and the stirring time is 0.5-2 h.

[0009] Specifically, in step (2), 10-30 mL of the sodium silicate solution with a concentration of 13-19 g / L obtained in step (1) and 0.4-0.6 g of the template agent can be added to 50-200 mL of water. Furthermore, in step (2), the flow rate of the CO2 gas can be 30-70 mL / min. The drying condition can be drying at 60°C for 24 h.

[0010] In the further step (2), the calcination process is: firstly heating to 200-300°C and keeping the temperature for 1-3 hours, and then heating to 500-600°C and keeping the temperature for 5-7 hours, in order to remove the template. The template includes but is not limited to one or more of hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, etc.

[0011] Further preferably, in step (2), the interval between the second additions of the sodium silicate solution is 1 h, 2 h, 3 h or 4 h; the amount of the second addition of the sodium silicate solution is 5 mL, 10 mL, 15 mL or 20 mL. That is, 5 mL, 10 mL, 15 mL or 20 mL of the sodium silicate solution can be added for the second time when the reaction is carried out for 1 h, 2 h, 3 h or 4 h.

[0012] Specifically, in step (3), the dispersant includes but is not limited to any one of methanol, ethanol and water; during the impregnation process, the dispersant serves to fully disperse the organic amine and the carrier in the system, so that the organic amine is gradually loaded into the pore structure of the carrier. When the dispersion is uniform, the stirrer can be stirred at 300-1200 rpm for 12-36 hours at room temperature to allow the dispersant to gradually evaporate.

[0013] Furthermore, in step (3), the organic amine includes but is not limited to any one of ethanolamine, polyethyleneimine, tetraethylenepentamine, polyacrylamide and pentaethylenehexamine, etc.; the organic amine preferably accounts for 30-65% of the mass of the multi-level porous solid amine adsorbent, such as 30 wt.%, 40 wt.%, 50 wt.%, 60 wt.% and 65 wt.%, etc. The vacuum drying temperature in the vacuum drying oven is 50-105°C, and the drying time is 12-24 h, until the dispersant is completely evaporated.

[0014] The present invention provides a fly ash-based controllable multi-level pore solid amine adsorbent prepared by the above method. The adsorbent obtained by the present invention has a rich pore structure and can reduce the mass transfer resistance during the CO2 adsorption process, thereby achieving high-value utilization of waste while increasing the adsorption capacity.

[0015] The present invention also provides the use of the above fly ash-based controllable multi-level porous solid amine adsorbent in CO2 capture.

[0016] The process of the present invention mainly includes two steps: 1) extracting silicon-rich solution from fly ash by alkaline leaching to synthesize a multi-level porous carrier; 2) modifying the multi-level porous SiO2 carrier with organic amine to prepare a multi-level porous solid amine adsorbent. In summary, compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The present invention develops a method for preparing a multi-level porous SiO2-based solid amine adsorbent using fly ash, a solid waste of coal-fired power plants, as a silicon source. The method can effectively utilize fly ash to extract silicon, solve the problem of resource waste and environmental harm of solid waste, and improve the cost-effectiveness of solid amine adsorbents.

[0017] (2) The present invention uses fly ash, a solid waste from coal-fired power plants, as raw material to significantly reduce the preparation cost of CO2 adsorbents. The pore structure of the SiO2 multi-level pore carrier is adjusted by template pore formation and interval self-assembly, which promotes the uniform dispersion of organic amines and improves the CO2 adsorption capacity. Low-cost, high-capacity solid amine adsorbents are promoted to the industrialization of CO2 capture technology, achieving the ideal goal of "treating waste with waste".

[0018] (3) The synthesis process of the present invention is relatively simple, the raw material cost is low, and it can meet the needs of large-scale industrial production, with economic value and social benefits. The present invention rationally designs the pore structure of the adsorbent carrier from the perspective of kinetics and thermodynamics. The preparation method and pore structure regulation process are safe and controllable. The synthesized multi-level porous SiO2 solid amine adsorbent has a high specific surface area and rich multi-level pore distribution. The -NH2 modified by wet impregnation can be highly dispersed in pores of different sizes, avoiding pore blockage and increasing CO2 mass transfer resistance, effectively improving the amine efficiency and being able to highly selectively adsorb CO2 in power plant flue gas. It is an effective way to develop high-efficiency CO2 adsorbents. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The SEM images of the multi-level porous SiO2 synthesized at different dosing intervals under the same dosing amount described in Examples 2-5 of the present invention, wherein in CS-xy, x: interval time y: secondary dosing amount; Figure 2 The pore size distribution diagram of the multi-level porous SiO2 synthesized at the same dosage and different dosage intervals in Examples 2-5 of the present invention; Figure 3 The SEM images of the multi-level porous SiO2 synthesized at different dosages at the same interval time described in Examples 6-9 of the present invention, wherein in CS-xy, x: interval time y: secondary dosage; Figure 4 The pore size distribution diagram of the multi-level porous SiO2 synthesized at different dosages at the same interval time described in Examples 6-9 of the present invention; Figure 5 The adsorption performance of solid amine adsorbent samples for CO2 synthesized at different intervals at the same dosage described in Examples 2-5 of the present invention; Figure 6 The adsorption performance of solid amine adsorbent samples synthesized with different secondary dosages at the same interval time described in Examples 6-9 of the present invention for CO2, CS is the mesoporous SiO2 carrier prepared in Example 1 without secondary dosage; Figure 7 The adsorption performance of CO2 by the solid amine adsorbent samples of the multi-level porous SiO2 synthesized in Example 10 of the present invention and impregnated with different amounts of organic amines; Figure 8 This is the CO2 saturated adsorption capacity of the multi-level porous SiO2 solid amine adsorbent synthesized in Example 10 of the present invention after ten adsorption and desorption cycle tests. DETAILED DESCRIPTION

[0020] In order to enable people in this research field to better understand the scheme of the present invention, the technical scheme in the embodiment of the present invention will be described in a complete and clear manner in combination with the drawings in the embodiment of the present invention. The specific embodiment is a detailed description of the present invention. Obviously, the described embodiment should be understood as only a further explanation of the present invention, rather than a specific limitation of the present invention. Any modification or replacement that does not depart from the technical scope of the present invention should be within the scope of protection of the rights claimed by the present invention.

[0021] In the following examples, unless otherwise specified, the raw materials used are commercially available products or can be prepared using conventional techniques in the art. Fly ash comes from solid waste from a coal-fired power plant. The calcination treatment of fly ash in the examples refers to calcination at 700°C for 2 h.

[0022] In the following Examples 1-10, the organic amine selected is pentaethylenehexamine (PEHA) and the dispersant selected is methanol.

[0023] Example 1 In this embodiment, a mesoporous SiO2 carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functionalization modification and mesoporous SiO2 carrier preparation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, mix with 5 g of sodium hydroxide, add 15 mL of deionized water, stir and heat to 110 °C for reaction, the reaction ends after 0.5 h, filter while hot, and obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: Add 25 mL of sodium silicate solution and 0.462 g of template to 80 mL of deionized water, heat and stir, introduce CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) into the reaction system at 70 °C for 5 h. After the reaction, filter the precipitate and dry it in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised to 250 °C at a rate of 5 °C / min and kept for 2 h, and then heated to 600 °C at the same rate and kept for 6 h to obtain a mesoporous SiO2 carrier (denoted as CS).

[0024] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared mesoporous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature and ventilation (stir at 800 rpm for about 24 h, the same below) to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for 24 h until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0025] Example 2 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / l; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for a total of 5 h. 15 mL of sodium silicate solution was added to the reaction system for a second time after 1 h of reaction. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same heating rate and kept for 6 h to obtain a multi-level porous SiO2 carrier (denoted as CS-1-15). The microscopic morphology of the carrier is shown in Figure 1 The pore size distribution is shown in Figure 2 As shown; Figure 1 It can be seen that the samples with the same dosage and different intervals are all composed of spherical particles and lamellar structures stacked and aggregated, and the proportions of spherical particles and lamellar structures in the samples with different intervals are different; Figure 2 It can be seen that the samples with the same dosage and different interval time show different pore size distributions, confirming the formation of a multi-level pore structure.

[0026] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature under ventilation to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0027] Example 3 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water, and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for a total of 5 h. 15 mL of sodium silicate solution was added to the reaction system for a second time after 2 h of reaction. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same heating rate and kept for 6 h to obtain a multi-level porous SiO2 carrier (denoted as CS-2-15). The microscopic morphology of the carrier is shown in FIG. Figure 1 The pore size distribution is shown in Figure 2 As shown; Figure 1 It can be seen that the samples with the same dosage and different intervals are all composed of spherical particles and lamellar structures stacked and aggregated, and the proportions of spherical particles and lamellar structures in the samples with different intervals are different; Figure 2 It can be seen that the samples with the same dosage and different interval time show different pore size distributions, confirming the formation of a multi-level pore structure.

[0028] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier into S4 to obtain an organic amine dispersion, and perform ultrasonic dispersion and mechanical stirring at room temperature and ventilation environment to gradually volatilize the dispersant; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0029] Example 4 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.% CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for a total of 5 h. 15 mL of sodium silicate solution was added to the reaction system for a second time when the reaction was carried out for 3 h. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same heating rate and kept for 6 h to obtain a multi-level porous SiO2 carrier (denoted as CS-3-15). The microscopic morphology of the carrier is shown in Figure 1 The pore size distribution is shown in Figure 2 As shown; Figure 1 It can be seen that the samples with the same dosage and different intervals are all composed of spherical particles and lamellar structures stacked and aggregated, and the proportions of spherical particles and lamellar structures in the samples with different intervals are different; Figure 2 It can be seen that the samples with the same dosage and different interval time show different pore size distributions, confirming the formation of a multi-level pore structure.

[0030] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature under ventilation to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0031] Example 5 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for a total of 5 h. 15 mL of sodium silicate solution was added to the reaction system for a second time when the reaction was carried out for 4 h. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same heating rate and kept for 6 h to obtain a multi-level porous SiO2 carrier (denoted as CS-4-15). The microscopic morphology of the carrier is shown in Figure 1 The pore size distribution is shown in Figure 2 As shown; Figure 1 It can be seen that the samples with the same dosage and different intervals are all composed of spherical particles and lamellar structures stacked and aggregated, and the proportions of spherical particles and lamellar structures in the samples with different intervals are different; Figure 2 It can be seen that the samples with the same dosage and different interval time show different pore size distributions, confirming the formation of a multi-level pore structure.

[0032] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature under ventilation to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0033] Example 6 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for 5 h, wherein 5 mL of sodium silicate solution was added to the reaction system for a second time after 1 h of reaction. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h; S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same heating rate and kept for 6 h to obtain a multi-level porous SiO2 carrier (denoted as CS-1-5). The microscopic morphology of the carrier is shown in Figure 3 The pore size distribution is shown in Figure 4 As shown; Figure 3 It can be seen that the number of lamellar structures in samples with different dosages at the same interval time increases with the increase of dosage, and the proportions of spherical particles and lamellar structures in samples with different dosages are different; Figure 4 It can be seen that the samples with different dosages at the same interval time show different pore size distributions, confirming the formation of a multi-level pore structure.

[0034] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature under ventilation to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0035] Example 7 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for a total of 5 h. 10 mL of sodium silicate solution was added to the reaction system for a second time after 1 h of reaction. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same heating rate and kept for 6 h to obtain a multi-level porous SiO2 carrier (denoted as CS-1-10). The microscopic morphology of the carrier is shown in Figure 3 The pore size distribution is shown in Figure 4 As shown; Figure 3 It can be seen that the number of lamellar structures in samples with different dosages at the same interval time increases with the increase of dosage, and the proportions of spherical particles and lamellar structures in samples with different dosages are different; Figure 4 It can be seen that the samples with different dosages at the same interval time show different pore size distributions, confirming the formation of a multi-level pore structure.

[0036] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature under ventilation to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0037] Example 8 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for a total of 5 h. 15 mL of sodium silicate solution was added to the reaction system for a second time after 1 h of reaction. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same heating rate and kept for 6 h to obtain a multi-level porous SiO2 carrier (CS-1-15). The microscopic morphology of the carrier is shown in FIG. Figure 3 The pore size distribution is shown in Figure 4 As shown; Figure 3 It can be seen that the number of lamellar structures in samples with different dosages at the same interval time increases with the increase of dosage, and the proportions of spherical particles and lamellar structures in samples with different dosages are different; Figure 4 It can be seen that the samples with different dosages at the same interval time show different pore size distributions, confirming the formation of a multi-level pore structure.

[0038] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature under ventilation to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0039] Example 9 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for a total of 5 h. 20 mL of sodium silicate solution was added to the reaction system for a second time after 1 h of reaction. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same heating rate and kept for 6 h to obtain a multi-level porous SiO2 carrier (denoted as CS-1-20). The microscopic morphology of the carrier is shown in FIG. Figure 3 The pore size distribution is shown in Figure 4 As shown; Figure 3 It can be seen that the number of lamellar structures in samples with different dosages at the same interval time increases with the increase of dosage, and the proportions of spherical particles and lamellar structures in samples with different dosages are different; Figure 4 It can be seen that the samples with different dosages at the same interval time show different pore size distributions, confirming the formation of a multi-level pore structure.

[0040] Organic amine modification: S4: Add a certain amount of organic amine into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain an organic amine dispersion; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature under ventilation to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (organic amine accounts for 50% of the mass of the solid amine adsorbent).

[0041] Example 10 In this embodiment, a multi-level pore structure carrier is prepared by the following steps, and the obtained solid amine adsorbent includes organic amine functional modification and carrier pore structure regulation: Preparation of fly ash-based SiO2 carrier: S1: Take 10 g of fly ash that has been calcined to remove organic matter and carbon deposits, stir and mix with 5 g of sodium hydroxide, add 15 mL of deionized water and heat to 110 °C for reaction. The reaction ends after 0.5 h, and filter while hot to obtain a sodium silicate solution with a concentration of 15.7 g / L; S2: 25 mL of sodium silicate solution and 0.462 g of template were added to 80 mL of deionized water, heated and stirred, and CO2 (CO2 / N2: 20 / 80 vol.%, CO2 gas flow rate of 50 mL / min) was introduced into the reaction system at 70 °C for a total of 5 h. 20 mL of sodium silicate solution was added to the reaction system for a second time after 1 h of reaction. After the reaction, the precipitate was filtered and dried in an oven at 60 °C for 24 h. S3: The dried product was ground and placed in a quartz boat, and calcined in a muffle furnace under air atmosphere. The temperature was raised at 5 °C / min to 250 °C and kept for 2 h. Then, it was heated to 600 °C at the same temperature and kept for 6 h to obtain a multi-level porous SiO2 carrier (denoted as CS-1-20).

[0042] Organic amine modification: S4: Add different masses of organic amines into 10 mL of dispersant methanol and stir for 0.5 h to dissolve to obtain organic amine dispersions; S5: Add 1 g of the prepared hierarchical porous SiO2 carrier to S4 to obtain an organic amine dispersion, and perform mechanical stirring at room temperature under ventilation to allow the dispersant to evaporate gradually; S6: After stirring until the dispersant is completely volatilized, place the sample in a 60 ℃ vacuum drying oven for vacuum drying for 24 hours until the dispersant is completely evaporated and the remaining solid matter is the solid amine adsorbent (the organic amine accounts for 30%, 40%, 50%, 60% and 65% of the mass of the solid amine adsorbent, respectively).

[0043] Evaluation of CO2 adsorption and cyclic stability This embodiment uses conventional test methods in the field, which can be referred to as follows: The CO2 adsorption performance of the sample is evaluated using a fixed bed reactor and an infrared gas analyzer (produced by Beijing Taihe Lianchuang Technology Co., Ltd., model: THA100S). 1 g of adsorbent was added to a quartz tube with an inner diameter of 1 cm for adsorption, analysis and cyclic testing of the sample. Before the test, the samples were pretreated in pure N2 (flow rate: 100 mL / min) at 120 °C for 0.5 h to remove the impurity gas adsorbed by the sample. Then the reaction system was cooled to the required test temperature (70 °C), and CO2 / N2 (CO2: N2=20 vol.% / 80vol.%) raw gas was passed into the reactor at a flow rate of 60 mL / min. The outlet gas concentration was monitored and recorded in real time by the gas analyzer. During the analysis process, the reaction temperature of the sample was raised to 120 °C and maintained for 0.5 h with N2 (100 mL / min). In the recycling experiment, the above adsorption-analysis processes were carried out alternately.

[0044] Figure 5 The adsorption performance of solid amine adsorbent samples synthesized at different intervals under the same dosage as described in Examples 2-5 of the present invention for CO2 is given. It can be seen from the figure that the adsorption capacity of the adsorbent CS-1-15 50PEHA with an interval of 1 h is 3.863 mmol / g, which is higher than the adsorbents with intervals of 2 h, 3 h, and 4 h, so the interval of 1 h is the best interval for secondary sample solution addition.

[0045] Figure 6 The adsorption performance of solid amine adsorbent samples synthesized with different secondary dosages at the same interval time described in Examples 6-9 of the present invention for CO2 is given, and CS is the mesoporous SiO2 carrier prepared without secondary dosage in Example 1. It can be seen from the figure that when the interval time is the same (1 h), the adsorption capacity of the adsorbent CS-1-2050PEHA prepared by secondary dosage of 20 mL of sodium silicate solution is 4.442 mmol / g, which is higher than the adsorbents with secondary dosages of 5 mL, 10 mL, and 15 mL, so the secondary dosage of 20 mL is the best secondary sample solution dosage.

[0046] Figure 7 The adsorption performance of solid amine adsorbent samples synthesized by impregnating CS-1-20 with different mass fractions of PEHA described in Example 10 of the present invention for CO2 is given. It can be seen from the figure that CS-1-20 60 PEHA has the highest adsorption capacity, the sample with low impregnation amount has a small number of adsorption active sites, and the sample with high impregnation amount is easy to block the pores. Therefore, the optimal amine impregnation amount is 60wt.% and is used for subsequent adsorption cyclic test.

[0047] Figure 8The saturated CO2 adsorption capacity of the multi-level porous SiO2 solid amine adsorbent synthesized in Example 10 of the present invention is given in ten adsorption and desorption cycle tests. Figure 8 The saturated CO2 adsorption amount of the solid amine adsorbent shown in the test process of ten adsorption and desorption cycles shows that: compared with other silicon-based solid amine adsorbents, the fly ash-based SiO2 solid amine adsorbent developed by the present invention has better CO2 adsorption performance, and the CO2 adsorption amount attenuation rate after 10 adsorption and desorption cycle tests is low. In addition, the current market price of fly ash from coal-fired power plants is 120.6 yuan / ton, which is much lower than synthetic silicon-based materials such as SiO2, SBA-15 molecular sieve and MCM-41 molecular sieve. Therefore, the fly ash-based multi-level porous SiO2 solid amine adsorbent developed by the present invention has the advantages of excellent adsorption performance, simple preparation method, low cost, and easy to scale up production, thereby showing good prospects for industrial application.

[0048] The applicant declares that although the present invention describes in detail the preparation method of a fly ash-based multi-level porous SiO2 solid amine adsorbent and its CO2 capture application through the above-mentioned embodiments, it is not limited to the above-mentioned specific operating steps. Other technical personnel in the field, inspired by the present invention, make modifications or substitutions to the present invention without departing from the concept of the present invention, which are all within the scope of protection of the present invention.

Claims

1. A method for preparing a fly ash-based controllable multi-level porous solid amine adsorbent, It is characterized in that The steps include: (1) Mix the fly ash calcined at high temperature with a certain amount of NaOH and water, and then stir and react at 110±20℃ for 0.5-3h. After the reaction is completed, filter and the filtrate is the sodium silicate solution; (2) Add the sodium silicate solution and template obtained in step (1) into water, heat and stir, and after the reaction temperature reaches 50-90°C, introduce a certain flow rate of CO 2 The gas reacts for 1-5 h. After the reaction is completed, the mesoporous SiO is obtained by filtration, drying and calcination. 2 Carrier; Alternatively, when CO is introduced 2 During the 1-5 h gas reaction, a certain amount of the sodium silicate solution obtained in step (1) is added twice at a certain interval. After the reaction is completed, the multi-level porous SiO 2 ; (3) Dissolve a certain amount of organic amine in the dispersant and then add the above-mentioned mesoporous SiO 2 Support or multi-level porous SiO 2 The mixture is dispersed evenly and dried after the dispersant evaporates to obtain a multi-level porous solid amine adsorbent.

2. The method for preparing the fly ash-based controllable multi-level porous solid amine adsorbent according to claim 1, It is characterized in that In step (1), the high temperature calcination temperature is 600-800°C, the high temperature calcination time is 2-4 h; and the mass ratio of fly ash to NaOH is 2-4:

1.

3. The method for preparing the fly ash-based controllable multi-level porous solid amine adsorbent according to claim 1, It is characterized in that In step (2), 10-30 mL of the sodium silicate solution with a concentration of 13-19 g / L obtained in step (1) and 0.4-0.6 g of the template are added to 50-200 mL of water.

4. The method for preparing the fly ash-based controllable multi-level porous solid amine adsorbent according to claim 1, It is characterized in that In step (2), CO is introduced 2 The gas flow rate was 30-70 mL / min.

5. The method for preparing the fly ash-based controllable multi-level porous solid amine adsorbent according to claim 1, It is characterized in that In step (2), the calcination process is: firstly raise the temperature to 200-300°C and keep it for 1-3 hours, then raise the temperature to 500-600°C and keep it for 5-7 hours.

6. The method for preparing the fly ash-based controllable multi-level porous solid amine adsorbent according to claim 1, It is characterized in that In step (2), the template is one or more of hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, and dodecyltrimethylammonium bromide.

7. The method for preparing the fly ash-based controllable multi-level porous solid amine adsorbent according to claim 1, It is characterized in that In step (2), the interval between the second additions of the sodium silicate solution is 1 h, 2 h, 3 h or 4 h; the amount of the second addition of the sodium silicate solution is 5 mL, 10 mL, 15 mL or 20 mL.

8. The method for preparing the fly ash-based controllable multi-level porous solid amine adsorbent according to claim 1, It is characterized in that In step (3), the dispersant is any one of methanol, ethanol and water; the organic amine is any one of ethanolamine, polyethyleneimine, tetraethylenepentamine, polyacrylamide and pentaethylenehexamine; and the organic amine accounts for 30-65% of the mass of the multi-level porous solid amine adsorbent.

9. A fly ash-based controllable multi-level porous solid amine adsorbent prepared by the method according to any one of claims 1 to 8.

10. The fly ash-based controllable multi-level porous solid amine adsorbent according to claim 9 is used in CO 2 Capture applications.

Citation Information

Patent Citations

  • Preparation method of solid amine gas adsorption material

    CN103785349A

  • Preparation method of silicon dioxide

    CN104418332A

  • Method for synthesizing ordered mesopore nano-silica through pulverous coal

    CN106517222A

  • Preparation method of mesoporous and microporous adsorption material for capturing carbon dioxide

    CN108816180A

  • Preparation method and application of aminated silica particle adsorbent

    CN110075812A

Cited By

  • Ammonia modified fly ash-based aerogel as well as preparation method and application thereof

    CN119771376A

  • Immersion process amine modified solid amine adsorbent and preparation method thereof

    CN121988306A