Preparation method of modified carbon black adsorbent for adsorbing heavy metals in wastewater and adsorbent
Through the preparation of modified carbon black adsorbent, the operational complexity and high cost problems in the treatment of heavy metal pollution in wastewater are solved, efficient adsorption of various heavy metals is achieved, secondary pollution is reduced, and cheap and efficient wastewater treatment is provided plan.
Patent Information
- Application Number
- CN202411353784.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has problems such as complex operation, high operating costs and secondary pollution when dealing with heavy metal pollution in wastewater, and lacks efficient adsorbent materials.
The modified carbon black adsorbent is prepared by mixing and calculating the carbon black raw material and pore-forming agent, and surface grafting modification is performed to prepare a modified carbon black adsorbent with a high specific surface area for adsorption of wastewater. Heavy metal ions.
It achieves good adsorption effect on a variety of heavy metal ions, reduces operational complexity and operating costs, and reduces secondary pollution, providing a cheap and efficient wastewater treatment solution.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of wastewater treatment, and in particular to a preparation method and an adsorbent of a modified carbon black adsorbent for adsorbing heavy metals in wastewater. Background Art
[0002] Water is one of the most important material resources that humans rely on for survival and development. However, with the rapid development of industrial and agricultural production and the economy, a large amount of wastewater containing pollutants is discharged into the environment without treatment, resulting in increasingly serious water pollution, further exacerbating the shortage of water resources and seriously threatening ecological security. Among the many water pollutions, heavy metal pollution accounts for a considerable proportion. Since heavy metals cannot be degraded and have enrichment, they can be transferred to animals or humans through the food chain, causing biological poisoning, and are classified as Class I pollutants. Faced with increasingly serious heavy metal pollution, which seriously threatens development, the treatment of heavy metal wastewater is imminent. After years of development, a variety of heavy metal treatment technologies have been formed, mainly including redox method, chemical precipitation method, ion exchange method, extraction method, chemical oxidation method, flocculation precipitation method and membrane filtration method. However, these treatment technologies have the disadvantages of complex operation process, high operating cost and secondary pollution. Adsorption separation method is the most active treatment method for removing toxic pollutants in sewage in recent years. The adsorption and separation function of adsorbent materials is to use porous solid compounds to effectively separate and enrich one or several components from multiple complex systems through physical or chemical methods. The adsorption method has the following characteristics in sewage treatment: 1) It can deeply treat wastewater containing extremely low concentrations of pollutants after chemical precipitation; 2) Many adsorbents can be reused through desorption methods such as acid washing and salt washing; 3) The variety of adsorbents used can meet the requirements of different application environments; 4) Secondary pollution is small. Adsorbents that can usually be used for water treatment include carbon adsorbents, biological adsorbents, minerals, silica gel and polymer adsorbents. In order to protect the ecological environment and reduce the harm caused by sewage, the development of adsorbent materials with better performance and more types is a topic that people should pay attention to at present. Summary of the invention
[0003] The present invention provides a preparation method of a modified carbon black adsorbent and an adsorbent for adsorbing heavy metals in wastewater to solve the deficiencies in the related art.
[0004] According to a first aspect of an embodiment of the present disclosure, there is provided a method for preparing a modified carbon black adsorbent for adsorbing heavy metals in wastewater, the preparation method comprising the following steps:
[0005] Step 1: providing a carbon black raw material, mixing the carbon black raw material with a pore-forming agent, and calcining at 300° C.-400° C. for 3-6 hours to obtain a porous carbon black material;
[0006] Step 2: The porous carbon black material is subjected to surface grafting modification to prepare the modified carbon black adsorbent.
[0007] In one aspect of the disclosed embodiment, step 1 includes:
[0008] Flour is mixed with water, and stirred to form a paste, and the carbon black raw material and pore-forming agent are added to the paste, and stirring is continued to obtain a mixture; the mixture is dried, and then calcined at 300° C.-400° C. for 3-6 hours to obtain the porous carbon black material.
[0009] In one aspect of the embodiments of the present disclosure, the mass ratio of the flour to the carbon black is selected from (0.35-0.75):1.
[0010] In one aspect of the embodiments of the present disclosure, in step 1, the pore-forming agent is selected from nitric acid. Preferably, the pore-forming agent is selected from 1-2 mol / L nitric acid solution.
[0011] In one aspect of the embodiments of the present disclosure, step 2 includes the following steps 2-1 and 2-2:
[0012] Step 2-1: using chloromethyl ethylene oxide to perform a first surface grafting modification on the porous carbon black material obtained in step 1 to obtain a porous carbon black material subjected to surface grafting treatment;
[0013] Step 2-2: Use polyethyleneimine to perform a second surface grafting modification on the porous carbon black material obtained in step 2-1 and subjected to surface grafting treatment, to obtain the modified carbon black adsorbent.
[0014] In one aspect of the disclosed embodiment, step 2-1 includes:
[0015] The chloromethyl ethylene oxide is added to methanol and stirred, and then the porous carbon black material obtained in step 1 is added, and tetrabutylammonium bromide is added while stirring is maintained, and the mixture is refluxed at 45° C.-55° C. for 3-4 hours to obtain a porous carbon black material with surface grafting treatment.
[0016] In one aspect of the embodiments of the present disclosure, in step 2-1, the mass of the chloromethyl oxirane is b1 mL, the mass of the porous carbon black material is b2 g, and b1 and b2 satisfy 5≤(b2 / b1)≤15.
[0017] In one aspect of the disclosed embodiment, in step 2-1, the mass of the chloromethyl oxirane is b1 mL, the mass of the porous carbon black material is b2 g, and b1 and b2 satisfy 5≤(b2 / b1)≤7.
[0018] In one aspect of the disclosed embodiment, step 2-2 includes:
[0019] The polyethyleneimine is dissolved in N,N-dimethylformamide, and the porous carbon black material obtained in step 2-1 and subjected to surface grafting treatment is added while stirring, and nitrogen is introduced for protection. The reaction is carried out at 65° C.-55° C. for 5-7 hours, and the product after the reaction is washed and dried to obtain the modified carbon black adsorbent.
[0020] In one aspect of an embodiment of the present disclosure, the present disclosure provides a method for preparing a modified carbon black adsorbent for adsorbing heavy metals in wastewater, the preparation method comprising the following steps:
[0021] Step 1: Mix flour and water, stir to form a paste, add the carbon black raw material and pore-forming agent to the paste, continue stirring to obtain a mixture; dry the mixture, and then calcine it at 300° C.-400° C. to obtain the porous carbon black material;
[0022] Step 2-1: Add chloromethyl ethylene oxide to methanol and stir, then add the porous carbon black material obtained in step 1, keep stirring and add tetrabutylammonium bromide, reflux at 45°C-55°C for 3-4h to obtain a porous carbon black material with surface grafting treatment;
[0023] Step 2-2: dissolve polyethyleneimine in N,N-dimethylformamide, keep stirring and add the porous carbon black material obtained in step 2-1 that has been surface grafted, pass nitrogen for protection, react at 65°C-75°C for 5-7h, wash and dry the reaction product to obtain the modified carbon black adsorbent.
[0024] According to a second aspect of an embodiment of the present disclosure, there is provided an adsorbent for adsorbing heavy metals in wastewater, wherein the adsorbent is prepared by the aforementioned preparation method.
[0025] The technical solution provided by the embodiments of the present disclosure may have the following beneficial effects:
[0026] It can be seen from the above embodiments that the present disclosure uses cheap carbon black as a raw material to prepare an adsorbent for adsorbing heavy metals in wastewater, and the adsorbent has a good adsorption effect on various heavy metal ions in wastewater.
[0027] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. DETAILED DESCRIPTION
[0028] Here, exemplary embodiments will be described in detail, and the implementations described in the following exemplary embodiments do not represent all implementations consistent with the present disclosure.
[0029] The terms used in this disclosure are for the purpose of describing specific embodiments only and are not intended to limit the disclosure. The singular forms of "a", "said" and "the" used in this disclosure and the appended claims are also intended to include plural forms unless the context clearly indicates otherwise. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.
[0030] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.
[0031] In this article, the terms "comprises", "comprising" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of more restrictions, an element defined by the sentence "comprising a ..." does not exclude the presence of other identical elements in the process, method, article or device that includes the element.
[0032] In the description herein, unless otherwise specified, “above” and “below” include the number.
[0033] Unless otherwise specified, the terms used in this disclosure have the well-known meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values of the various parameters mentioned in this disclosure can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this disclosure).
[0034] The term "about" is used to describe and illustrate small changes. When used in conjunction with an event or situation, the term may refer to an example in which the event or situation occurs precisely and an example in which the event or situation occurs very approximately. For example, when used in conjunction with a numerical value, the term may refer to a range of variation of less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. In addition, amounts, ratios, and other numerical values are sometimes presented in this article in a range format. It should be understood that such a range format is for convenience and simplicity, and should be flexibly understood to include not only numerical values explicitly designated as range limits, but also all individual numerical values or subranges encompassed within the range, as if each numerical value and subrange were explicitly designated.
[0035] In the present disclosure, the carbon black raw material is selected from any one of carbon black N134, carbon black N110, carbon black N115, carbon black N121, carbon black N166, carbon black N219, carbon black N220, carbon black N231, carbon black N234, carbon black N242, carbon black N270, carbon black N285, carbon black N293, carbon black N294, carbon black N299, carbon black N326, carbon black N330, carbon black N332, carbon black N339, carbon black N347, carbon black N351, carbon black N356, carbon black N358, carbon black N363 or carbon black N375; preferably, the carbon black raw material used in the present disclosure is selected from carbon black N134.
[0036] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0037] In the present disclosure, step 1 includes: providing a carbon black raw material, mixing the carbon black raw material with a pore-forming agent, and then roasting at 300°C-400°C for 3-6 hours to obtain a porous carbon black material; specifically, step 1 includes: mixing flour with water, stirring to form a paste, adding the carbon black raw material and the pore-forming agent to the paste, and continuing to stir to obtain a mixture; drying the mixture, and then roasting at 300°C-400°C for 3-6 hours to obtain a porous carbon black material; further specifically, step 1 includes: mixing flour with a small amount of The mixture is mixed with water and stirred to form a paste, and a carbon black raw material and a pore-forming agent are added to the paste, wherein the mass ratio of flour to carbon black is selected from (0.35-0.75):1, the pore-forming agent is selected from 1-2 mol / L nitric acid solution, and the mass ratio of nitric acid solution to carbon black is selected from (0.8-1.5):1, and stirring is continued to obtain a mixture, which is also a paste; the mixture is dried at 55°C for 2-6h to obtain a dry mixture, and then the mixture is calcined at 320°C for 4h to obtain a porous carbon black material.
[0038] In the present disclosure, the purpose of step 1 is to prepare a loose and porous porous carbon black material, whose larger specific surface area is conducive to the adsorption of heavy metal ions; in addition, HNO3 is used as a pore-forming agent, which can not only undergo an oxidation reaction with the carbon atoms of the carbon black material at high temperature to consume part of the carbon atoms, thereby forming a loose and rough surface, but also, since the surface of carbon black carries groups such as -H, -OH and -COOH, HNO3 can further convert the -H and -OH groups on the surface of carbon black into -COOH groups at high temperature, thereby increasing reaction sites for the reactions of steps 2-1 and 2-2.
[0039] In the present disclosure, step 2-1 includes: using chloromethyl ethylene oxide to perform a first surface grafting modification on the porous carbon black material obtained in step 1 to obtain a porous carbon black material subjected to surface grafting treatment; specifically, step 2-1 includes: adding chloromethyl ethylene oxide to methanol and stirring, then adding the porous carbon black material obtained in step 1, keeping stirring and adding tetrabutylammonium bromide, and reflux reaction at 45°C-55°C for 3-4h to obtain a porous carbon black material subjected to surface grafting treatment; further specifically, step 2-1 includes: adding chloromethyl ethylene oxide to methanol and stirring, then adding the porous carbon black material obtained in step 1, keeping stirring and adding tetrabutylammonium bromide, wherein the amount of chloromethyl ethylene oxide used is b1 mL, and the mass of the porous carbon black material is b2 g, b1 and b2 satisfy 5≤(b2 / b1)≤15, the mass of tetrabutylammonium bromide added is 1wt%-5wt% of the mass of the porous carbon black material, and reflux reaction is carried out at 50°C for 3.5h to obtain a porous carbon black material with surface grafting treatment.
[0040] In the present disclosure, the purpose of step 2-1 is to graft the -COOH group on the surface of carbon black, and its chemical reaction formula is as follows (in the present disclosure, CB represents carbon black):
[0041]
[0042] In the present disclosure, step 2-2 includes: using polyethyleneimine (PEI) to perform a second surface grafting modification on the porous carbon black material obtained in step 2-1 and subjected to surface grafting treatment, to obtain a modified carbon black adsorbent; specifically, dissolving polyethyleneimine in N,N-dimethylformamide, stirring and adding the porous carbon black material obtained in step 2-1 and subjected to surface grafting treatment, introducing nitrogen for protection, reacting at 65°C-75°C for 5-7h, and washing and drying the product after the reaction to obtain the modified carbon black adsorbent; further specifically, dissolving a1 mL of polyethyleneimine in N,N-dimethylformamide, stirring and adding a2 g of the porous carbon black material obtained in step 2-1 and subjected to surface grafting treatment, wherein the value of a2 / a1 is selected from 0.3-1, introducing nitrogen for protection, reacting at 70°C for 6h, and washing and drying the product after the reaction to obtain the modified carbon black adsorbent.
[0043] In the present disclosure, the purpose of step 2-2 is to further modify the surface of carbon black, and its chemical reaction formula is as follows:
[0044]
[0045] In the present disclosure, since polyethyleneimine molecules have a large number of primary amine, secondary amine and tertiary amine groups, they have a strong chelating effect with heavy metal ions. Therefore, the carbon black material modified by grafting with chloromethyl ethylene oxide and polyethyleneimine can have a good adsorption effect on various heavy metal ions in wastewater.
[0046] The present invention is further described below by way of specific examples. The various chemical reagents used in the examples of the present invention are obtained through conventional commercial channels unless otherwise specified. Unless otherwise specified, the contents described below are all weight contents. Unless otherwise specified, it is understood that the process is carried out at room temperature.
[0047] Example:
[0048] Embodiment 1:
[0049] Embodiment 1 comprises the following steps:
[0050] Mix 5 g of flour with 25 mL of water and stir to form a paste. Add 10 g of carbon black N134 powder to the paste and continue stirring. Then add 10 mL of the prepared 2 mol / L dilute nitric acid and continue stirring to obtain a mixed paste. During the aforementioned stirring process, a small amount of water can be added appropriately. Dry the mixed paste at 55°C for 4 h to obtain a dry mixture, which is then calcined at 320°C for 4 h. Wash and dry the calcined product to obtain a porous carbon black material.
[0051] Weigh 2 mL of chloromethyl ethylene oxide, add it to 50 mL of methanol, continue stirring, then weigh 10 g of the porous carbon black material prepared above, add it to methanol, then add 0.3 g of tetrabutylammonium bromide, reflux at 50°C for 3.5 hours, filter, wash and dry the product after the reaction to obtain a porous carbon black material with surface grafting treatment.
[0052] Weigh 10 mL of polyethyleneimine, add it to 20 mL of DMF, keep stirring, weigh 5 g of porous carbon black material with surface grafting treatment, pass nitrogen for protection, react at 70 ° C for 6 hours, and then filter to obtain a solid product. The solid product is washed with water, alcohol, water, and dried to obtain the modified carbon black adsorbent of Example 1.
[0053] Embodiment 2:
[0054] Embodiment 2 comprises the following steps:
[0055] Mix 5g of flour with 25mL of water and stir to form a paste. Add 10g of carbon black N134 powder to the paste and continue stirring. Then add 10mL of the prepared 2mol / L (NH4)2CO3 solution and continue stirring to obtain a mixed paste. During the above stirring process, a small amount of water can be added appropriately. Dry the mixed paste at 55°C for 4h to obtain a dry mixture, and then calcine it at 320°C for 4h. Wash and dry the calcined product to obtain a porous carbon black material.
[0056] Weigh 2 mL of chloromethyl ethylene oxide, add it to 50 mL of methanol, continue stirring, then weigh 10 g of the porous carbon black material prepared above, add it to methanol, then add 0.3 g of tetrabutylammonium bromide, reflux at 50°C for 3.5 hours, filter, wash and dry the product after the reaction to obtain a porous carbon black material with surface grafting treatment.
[0057] Weigh 10 mL of polyethyleneimine, add it to 20 mL of DMF, keep stirring, weigh 5 g of porous carbon black material that has been surface grafted, pass nitrogen for protection, react at 70 ° C for 6 hours, and then filter to obtain a solid product. The solid product is washed with water, alcohol, water, and dried to obtain the modified carbon black adsorbent of Example 2.
[0058] Embodiment 3:
[0059] The steps of Example 3 are the same as those of Example 2, except that KOH is used instead of (NH4)2CO3 as the pore-forming agent.
[0060] Embodiment 4:
[0061] The steps of Example 4 are the same as those of Example 2, except that K2CO3 is used instead of (NH4)2CO3 as the pore former.
[0062] Embodiment 5:
[0063] Embodiment 5 comprises the following steps:
[0064] Mix 5 g of flour with 25 mL of water and stir to form a paste. Add 10 g of carbon black N134 powder to the paste and continue stirring. Then add 10 mL of the prepared 2 mol / L dilute nitric acid and continue stirring to obtain a mixed paste. During the aforementioned stirring process, a small amount of water can be added appropriately. Dry the mixed paste at 55°C for 4 h to obtain a dry mixture, which is then calcined at 320°C for 4 h. Wash and dry the calcined product to obtain a porous carbon black material.
[0065] Weigh 1.5 mL of chloromethyl ethylene oxide, add it to 50 mL of methanol, continue stirring, then weigh 10 g of the porous carbon black material prepared above, add it to methanol, then add 0.3 g of tetrabutylammonium bromide, reflux at 50°C for 3.5 hours, filter, wash and dry the product after the reaction to obtain a porous carbon black material with surface grafting treatment.
[0066] Weigh 10 mL of polyethyleneimine, add it to 20 mL of DMF, keep stirring, weigh 5 g of porous carbon black material that has been surface grafted, pass nitrogen for protection, react at 70 ° C for 6 hours, and then filter to obtain a solid product. The solid product is washed with water, alcohol, water, and dried to obtain the modified carbon black adsorbent of Example 5.
[0067] Embodiment 6:
[0068] The steps of Example 6 are the same as those of Example 5, except that 700 μL of chloromethyl oxirane is weighed instead of 1.5 mL of chloromethyl oxirane.
[0069] Embodiment 7:
[0070] The steps of Example 7 are the same as those of Example 5, except that 350 μL of chloromethyl oxirane is weighed instead of 1.5 mL of chloromethyl oxirane.
[0071] Embodiment 8:
[0072] The steps of Example 8 are the same as those of Example 5, except that 4 mL of chloromethyl oxirane is weighed instead of 1.5 mL of chloromethyl oxirane.
[0073] Comparative Example 1:
[0074] Comparative Example 1 comprises the following steps:
[0075] Weigh 2 mL of chloromethyl ethylene oxide, add it to 50 mL of methanol, continue stirring, then weigh 10 g of washed and dried carbon black N134 powder, add it to methanol, then add 0.3 g of tetrabutylammonium bromide, reflux at 50°C for 3.5 hours, filter, wash and dry the product to obtain a carbon black material with surface grafting treatment.
[0076] Weigh 10 mL of polyethyleneimine, add it to 20 mL of DMF, keep stirring, weigh 5 g of carbon black material with surface grafting treatment, pass nitrogen for protection, react at 70 ° C for 6 hours, and then filter to obtain a solid product. The solid product is washed with water, alcohol, water, and dried respectively to obtain the modified carbon black adsorbent of Comparative Example 1.
[0077] Comparative Example 2:
[0078] Comparative Example 2 comprises the following steps:
[0079] 10 g of washed and dried carbon black N134 powder was added to 100 mL of prepared 5 mol / L nitric acid, stirred and heated at 80° C. for 8 h, and the reaction product was washed and dried to obtain a carbon black material treated with nitric acid.
[0080] Weigh 2 mL of chloromethyl ethylene oxide, add it to 50 mL of methanol, continue stirring, then weigh 10 g of the carbon black material treated with nitric acid prepared above, add it to methanol, then add 0.3 g of tetrabutylammonium bromide, reflux at 50°C for 3.5 hours, filter, wash and dry the product after the reaction to obtain a carbon black material with surface grafting treatment.
[0081] Weigh 10 mL of polyethyleneimine, add it to 20 mL of DMF, keep stirring, weigh 5 g of carbon black material with surface grafting treatment, pass nitrogen for protection, react at 70 ° C for 6 hours, and then filter to obtain a solid product. The solid product is washed with water, alcohol, water, and dried to obtain the modified carbon black adsorbent of Comparative Example 2.
[0082] Comparative Example 3:
[0083] Comparative Example 3 comprises the following steps:
[0084] Mix 5 g of flour with 25 mL of water and stir to form a paste. Add 10 g of carbon black N134 powder to the paste and continue stirring. Then add 10 mL of the prepared 2 mol / L dilute nitric acid and continue stirring to obtain a mixed paste. During the aforementioned stirring process, a small amount of water can be added appropriately. Dry the mixed paste at 55°C for 4 h to obtain a dry mixture, which is then calcined at 320°C for 4 h. Wash and dry the calcined product to obtain a porous carbon black material.
[0085] Weigh 2 mL of chloromethyl ethylene oxide, add it to 50 mL of methanol, continue stirring, then weigh 10 g of the porous carbon black material prepared above, add it to methanol, then add 0.3 g of tetrabutylammonium bromide, reflux at 50°C for 3.5 hours, filter, wash and dry the product after the reaction to obtain a porous carbon black material with surface grafting treatment, and use the prepared porous carbon black material with surface grafting treatment directly as the carbon black adsorbent of Comparative Example 3.
[0086] Comparative Example 4:
[0087] Comparative Example 4 comprises the following steps:
[0088] Mix 5 g of flour with 25 mL of water and stir to form a paste. Add 10 g of carbon black N134 powder to the paste and continue stirring. Then add 10 mL of the prepared 2 mol / L dilute nitric acid and continue stirring to obtain a mixed paste. During the aforementioned stirring process, a small amount of water can be added appropriately. Dry the mixed paste at 55°C for 4 h to obtain a dry mixture, which is then calcined at 320°C for 4 h. Wash and dry the calcined product to obtain a porous carbon black material.
[0089] Weigh 10 mL of polyethyleneimine, add it to 20 mL of DMF, keep stirring, weigh 5 g of the prepared porous carbon black material, pass nitrogen for protection, react at 70 ° C for 6 hours, and then filter to obtain a solid product. The solid product is washed with water, washed with alcohol, washed with water, and dried to obtain the carbon black adsorbent of Comparative Example 4.
[0090] Heavy metal ion adsorption test:
[0091] Cu 2+ Adsorption test: Weigh 0.5 g of the modified carbon black adsorbent prepared in Examples 1-8 and add it to 100 mL of a 100 mg·L -1 Cu 2+ In solution, use 250r·min -1 After a certain period of constant temperature oscillation adsorption, the filtrate was taken and the remaining Cu in the solution was determined by ICP. 2+ Concentration, the removal rate is calculated as follows:
[0092] Removal rate (%) = (C0-C e ) / C0×100, where C e Cu in the final solution 2+ Concentration (mg·L -1 ); C0 is the initial Cu 2+ Concentration (mg·L -1 ).
[0093] Pb 2+ Adsorption test: Weigh 0.5 g of the modified carbon black adsorbent prepared in Examples 1-8 and add it to 100 mL of a 100 mg·L -1 Pb 2+ In solution, use 250r·min -1 After a certain period of constant temperature oscillation adsorption, the filtrate was taken and the remaining Pb in the solution was determined by ICP. 2+ Concentration, the removal rate is calculated as follows:
[0094] Removal rate (%) = (C0-C e ) / C0×100, where C e Pb in the final solution 2+ Concentration (mg·L -1 ); C0 is the initial Pb in the solution 2+ Concentration (mg·L -1 ).
[0095] Cd 2+ Adsorption test: Weigh 0.5 g of the modified carbon black adsorbent prepared in Examples 1-8 and add it to 100 mL of a 100 mg·L -1 CD 2+ In solution, use 250r·min -1 After a certain period of constant temperature oscillation adsorption, the filtrate was taken and the remaining Cd in the solution was determined by ICP. 2+ Concentration, the removal rate is calculated as follows:
[0096] Removal rate (%) = (C0-C e) / C0×100, where C e is the Cd content in the final solution 2+ Concentration (mg·L -1 ); C0 is the initial Cd in the solution 2+ Concentration (mg·L -1 ).
[0097] The adsorption test results of the above heavy metal ions are shown in Table 1:
[0098] Table 1
[0099]
[0100]
[0101] As can be seen from Table 1, the carbon black adsorbent containing a large number of primary amine, secondary amine and tertiary amine groups prepared in the present disclosure has a good effect on Cu 2+ , Pb 2+ and Cd 2+ All of them have good adsorption capacity. By comparing Example 1 with Examples 2-4, it can be seen that compared with other pore-forming agents, HNO3 can consume part of the carbon atoms to further increase the specific surface area, and HNO3 can further convert the -H and -OH groups on the surface of carbon black into -COOH groups at high temperature, thereby increasing the reaction sites for subsequent reactions. Therefore, HNO3 is the best pore-forming agent. By comparing Example 1 with Examples 5-8, it can be seen that when the amount of chloromethyl oxirane and the mass of the porous carbon black material meet a certain proportional relationship, the obtained adsorbent has a better adsorption effect. When the amount of chloromethyl oxirane is too little (Examples 6-7), the grafting reaction of chloromethyl oxirane is insufficient. When the amount of chloromethyl oxirane is too much (Example 8), the prepared carbon black is grafted with too many oxirane groups and polyethyleneimine groups, which have a large steric hindrance, but are not conducive to the adsorption of metal ions, especially metal ions with a larger radius (Pb 2+ ).
[0102] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the disclosure disclosed herein. The present disclosure is intended to cover any variations, uses or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure.
Claims
1. A method for preparing a modified carbon black adsorbent for adsorbing heavy metals in wastewater, characterized in that: The preparation method comprises the following steps: Step 1: providing a carbon black raw material, mixing the carbon black raw material with a pore-forming agent, and calcining at 300° C.-400° C. for 3-6 hours to obtain a porous carbon black material; Step 2: The porous carbon black material is subjected to surface grafting modification to prepare the modified carbon black adsorbent.
2. The preparation method according to claim 1, characterized in that: Step 1 includes: Flour is mixed with water, and stirred to form a paste, and the carbon black raw material and pore-forming agent are added to the paste, and stirring is continued to obtain a mixture; the mixture is dried, and then calcined at 300° C.-400° C. for 3-6 hours to obtain the porous carbon black material.
3. The preparation method according to claim 2, characterized in that: In step 1, the pore former is selected from nitric acid.
4. The preparation method according to claim 1, characterized in that: Step 2 includes the following steps 2-1 and 2-2: Step 2-1: using chloromethyl ethylene oxide to perform a first surface grafting modification on the porous carbon black material obtained in step 1 to obtain a porous carbon black material subjected to surface grafting treatment; Step 2-2: Use polyethyleneimine to perform a second surface grafting modification on the porous carbon black material obtained in step 2-1 and subjected to surface grafting treatment, to obtain the modified carbon black adsorbent.
5. The preparation method according to claim 4, characterized in that: Step 2-1 includes: The chloromethyl ethylene oxide is added to methanol and stirred, and then the porous carbon black material obtained in step 1 is added, and tetrabutylammonium bromide is added while stirring is maintained, and the mixture is refluxed at 45° C.-55° C. for 3-4 hours to obtain a porous carbon black material with surface grafting treatment.
6. The preparation method according to claim 5, characterized in that: In step 2-1, the mass of the chloromethyl oxirane is b1 mL, the mass of the porous carbon black material is b2 g, and b1 and b2 satisfy 5≤(b2 / b1)≤15.
7. The preparation method according to claim 4, characterized in that: Step 2-2 includes: The polyethyleneimine is dissolved in N,N-dimethylformamide, and the porous carbon black material obtained in step 2-1 and subjected to surface grafting treatment is added while stirring, and nitrogen is introduced for protection. The reaction is carried out at 65° C.-75° C. for 5-7 hours, and the product after the reaction is washed and dried to obtain the modified carbon black adsorbent.
8. An adsorbent for adsorbing heavy metals in wastewater, characterized in that: The adsorbent is prepared by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Novel heavy metal adsorbent mainly prepared from shrimp shells and preparation method thereof
CN102000552A
Preparation method and application of novel microporous starch
CN107433189A
Preparation method of magnetic cellulose-based polyamine chelating heavy metal adsorbent
CN115888664A
Modified biochar for treating acidic molybdenum-containing wastewater and preparation method of modified biochar
CN117299102A
Wastewater adsorbent, and preparation method therefor and use thereof
US20240367140A1
Cited By
Preparation process of high-adsorbability carbon black
CN120189918A