Preparation method, product and application of graphene oxide composite nanomaterial
The GO@PAA@Fe3O4 composite addresses separation and adsorption challenges by enhancing the stability and adsorption performance of GO@Fe3O4 through surface modification, achieving efficient extraction of indole compounds.
Patent Information
- Application Number
- CN202411380452.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Graphene oxide (GO) materials are difficult to separate from sample solutions due to their lightweight nature, and GO@Fe3O4 composites suffer from insufficient adsorption performance and structural instability during ultrasonic treatment.
A method involving EDC-NHS coupling to activate the -COOH group of GO with polyacrylamine (PAA) followed by co-precipitation with iron salts to form GO@PAA@Fe3O4, then activating with an acidic acetone solution to enhance stability and adsorption performance.
The resulting GO@PAA@Fe3O4 composite exhibits fast separation, high adsorption capacity, and strong stability, effectively adsorbing indole-3-acetic acid and indole-3-propionic acid with improved extraction efficiency.
Smart Images

Figure CN119075946A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of graphene oxide material preparation, and in particular to a preparation method, product and application of a graphene oxide composite nanomaterial. Background Art
[0002] With the continuous advancement of analytical detection technology, magnetic solid-phase extraction (MSPE) has attracted widespread attention in recent years due to its high extraction efficiency and large contact area. In the MSPE process, magnetic adsorbents play a key role, not only affecting the extraction efficiency, but also determining the sensitivity and selectivity of the detection method. Therefore, the development of magnetic adsorbents with high adsorption capacity has become a research focus. Graphene oxide (GO) has shown great potential in the field of adsorption due to its large specific surface area, light weight, fast mass transfer rate, and rich binding sites on the surface. The two main characteristics of GO are: (1) its structure contains a large number of freely movable π electrons; (2) its surface and edges are rich in oxidized functional groups, such as carboxyl (-COOH), hydroxyl (-OH) and epoxy groups. These characteristics make GO highly active in the adsorption process. At present, some studies have used GO as an adsorbent to successfully extract indole-3-acetic acid (IAA) and indole-3-propionic acid (IPA) from different plant matrices. However, GO also has some shortcomings. Due to its extremely light weight, it is still difficult to separate GO from the sample solution or extraction solution even under high-speed centrifugation conditions. In addition, there are strong π-π interactions between GO sheets, which easily lead to their aggregation or accumulation, thereby reducing the effective specific surface area and lowering the adsorption capacity.
[0003] In order to overcome these problems, Fe3O4 is often introduced into GO to form GO@Fe3O4 composite materials. Fe3O4 has the advantages of strong magnetism, low toxicity, low cost and easy preparation. Modifying Fe3O4 on the surface of GO can effectively improve its separation performance. However, studies have shown that the introduction of Fe3O4 does not significantly increase the active functional groups of GO. In addition, when Fe3O4 binds to the GO surface, it consumes the oxygen-containing functional groups in GO and affects the adsorption performance. More importantly, Fe3O4 exposed on the GO surface is easy to fall off during ultrasonic treatment, destroying the overall structure of the material, thereby limiting its practical application. Summary of the invention
[0004] Based on the above content, the present invention provides a preparation method, product and application of graphene oxide composite nanomaterials to solve the problem that GO materials are difficult to separate and GO@Fe3O4 has insufficient adsorption performance in the prior art. The graphene oxide composite nanomaterial of the present invention has the characteristics of fast separation speed, high adsorption performance and strong stability.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is a method for preparing a graphene oxide composite nanomaterial, comprising the following steps:
[0007] Step 1: According to the EDC-NHS coupling reaction, the -COOH group on GO (graphene oxide) is activated and coupled with the -NH2 of PAA (polyacrylamine) to form an amide bond to obtain GO@PAA;
[0008] Step 2, using iron salt and GO@PAA to prepare magnetic GO@PAA (N-GO@PAA@Fe3O4) by co-precipitation method;
[0009] Step 3, using an acidic acetone solution to activate the magnetic GO@PAA and wash it to obtain graphene oxide composite nanomaterials (GO@PAA@Fe3O4).
[0010] The second technical solution of the present invention is a graphene oxide composite nanomaterial prepared according to the above-mentioned preparation method.
[0011] The third technical solution of the present invention is the application of the above-mentioned graphene oxide composite nanomaterial in the adsorption of indole-3-acetic acid and indole-3-propionic acid.
[0012] The present invention discloses the following technical effects:
[0013] The present invention prepares a novel graphene oxide composite nanomaterial GO@PAA@Fe3O4 by a two-step method, which solves the problem that GO materials are difficult to separate and GO@Fe3O4 is insufficient in adsorption performance in the prior art. It also has a good adsorption effect on indole-3-acetic acid (IAA) and indole-3-propionic acid (IPA), solving the problems of low extraction rate of indole compounds and complex analysis methods. It is of great value for synthesizing nanomaterials with high adsorption performance and for rapid and efficient extraction and enrichment of target compounds, and has wide applicability.
[0014] The present invention successfully solves the problem that graphene oxide (GO) nanomaterials with high adsorption properties are difficult to separate from the test solution due to their ultra-light properties; in the process of Fe3O4 bonding with GO, a large number of oxygen-containing functional groups on GO are consumed, resulting in a significant reduction in adsorption performance, and the exposed Fe3O4 on the surface of GO is easy to fall off during the ultrasonic process. It greatly fills the gap in the existing field of synthesis of nanocomposite materials with high adsorption properties, with good separation effect, strong adsorption performance and strong stability, and provides a reliable tool for the rapid enrichment of the target, which has important scientific research value and application prospects. It also provides theoretical support for magnetic solid phase extraction technology, especially for indole-3-acetic acid (IAA) and indole-3-propionic acid (IPA).
[0015] The graphene oxide composite nanomaterial GO@PAA@Fe3O4 prepared by the present invention has the advantages of superparamagnetism and easy separation, dense adsorption sites showing high adsorption performance, good thermal stability and low cost, and has excellent performance and potential as an adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 The synthesis route of graphene oxide composite nanomaterial GO@PAA@Fe3O4: A self-assembly of polyacrylamine; B preparation of magnetic GO@PAA;
[0018] Figure 2 TEM images (AC) and SEM images (DF) of GO, GO@PAA and GO@PAA@Fe3O4;
[0019] Figure 3 Infrared spectra of GO, GO@PAA and GO@PAA@Fe3O4;
[0020] Figure 4 This is the XPS full scan spectrum of GO@PAA@Fe3O4;
[0021] Figure 5 High-resolution spectra of (A) C 1s, (B) O 1s, (C) N 1s and (D) Fe 2p of GO@PAA@Fe3O4;
[0022] Figure 6 is the zeta potential of GO and GO@PAA@Fe3O4;
[0023] Figure 7 Thermogravimetric curves of GO, GO@PAA and GO@PAA@Fe3O4;
[0024] Figure 8 The hysteresis loop of GO@PAA@Fe3O4 at 27°C. The lower right corner is in the range of -100 to 100 Oe;
[0025] Fig. 9The adsorption kinetics of (a in A) IAA and (a in B) IPA on GO@PAA@Fe3O4; the inset is the pseudo-first-order kinetic model of (b in A) IAA and (b in B) IPA fitted by Origin9.2, and the pseudo-second-order kinetic model of (c in A) IAA and (c in B) IPA;
[0026] Fig.10 Comparison of the Langmuir isotherm adsorption model (A, B) and the Freundlich isotherm adsorption model (C, D) for the adsorption of IAA and IPA on GO@PAA@Fe3O4. DETAILED DESCRIPTION
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0028] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0032] The "room temperature" described in the present invention, unless otherwise specified, refers to 15-35°C.
[0033] In order to solve the deficiencies of the adsorption performance of GO@Fe3O4 composite materials in the prior art, the present invention modifies the surface of the GO@Fe3O4 composite material. Specifically, the present invention uses an amino polymer polyacrylamine (PAA) to coat GO@Fe3O4, thereby effectively improving the stability and adsorption performance of the material. PAA can not only provide a high density of amino sites, but also form a stable bond with the target organic matter through hydrogen bonding, greatly improving the adsorption capacity and selectivity of the composite material.
[0034] The first aspect of the present invention provides a method for preparing a graphene oxide composite nanomaterial, comprising the following steps:
[0035] Step 1: According to the EDC-NHS coupling reaction, the -COOH group on GO (graphene oxide) is activated and coupled with the -NH2 of PAA (polyacrylamine) to form an amide bond to obtain GO@PAA;
[0036] Step 2, using iron salt and GO@PAA to prepare magnetic GO@PAA (N-GO@PAA@Fe3O4) by co-precipitation method;
[0037] Step 3, using an acidic acetone solution to activate the magnetic GO@PAA and wash it to obtain graphene oxide composite nanomaterials (GO@PAA@Fe3O4).
[0038] In a preferred embodiment of the present invention, in step 1, PAA is dissolved in buffer solution 1 (potassium phosphate buffer, pH=6-8) to obtain a PAA solution; EDC and NHS are sequentially added to a buffer solution 2 (MES buffer solution, pH=5.5-6.5) in which GO powder is dissolved for activation to obtain GO-EDC-NHS; the PAA solution and the GO-EDC-NHS are mixed and stirred for reaction to obtain GO@PAA.
[0039] In a preferred embodiment of the present invention, the mass ratio of the GO to the PAA is 1:15. The mass ratio of the EDC to NHS is 2:3; and the mass ratio of the GO to the EDC is 1:3.2.
[0040] In the present invention, the mass ratio of GO to EDC is limited to the above ratio for the following reasons: GO exceeding the ratio will lead to insufficient activation; EDC exceeding the ratio may lead to reduced coupling efficiency, increased by-products and reduced material stability due to over-activation.
[0041] In a preferred embodiment of the present invention, in step 2, after dispersing the GO@PAA in water, the GO@PAA is added to an acidic solution containing an iron salt and mixed, and then an ammonia solution is added to react to obtain magnetic GO@PAA.
[0042] In a preferred embodiment of the present invention, the iron salt is a mixture of a divalent iron salt and a trivalent iron salt; the molar ratio of the divalent iron salt to the trivalent iron salt is 1:2; the acidic solution is a 0.2-0.6 mol / L HCl solution. The divalent iron salt is FeCl2·4H2O; the trivalent iron salt is FeCl3·6H2O.
[0043] In a preferred embodiment of the present invention, the mass ratio of the iron salt to the GO@PAA is 12-13:1.
[0044] In a preferred embodiment of the present invention, the reaction is specifically carried out at a pH of 10-12 and a temperature of 85-95° C. for 3.5-5.5 hours.
[0045] In the present invention, when the pH is lower than 10, the ammonia water is insufficient to provide sufficient OH- ions, so that the coprecipitation reaction of the iron salt cannot be fully carried out, and the Fe3O4 particles may not be completely generated or the generated Fe3O4 particles are small, resulting in weakened magnetic properties of the material. At a lower pH value, the incompletely reacted Fe 3+ Byproducts such as iron hydroxide (Fe(OH)3) may be formed instead of the desired Fe3O4, affecting the purity and magnetic properties of the material;
[0046] When the pH value is too high, the OH- ion concentration is too large and the reaction rate is too fast, resulting in the rapid precipitation of Fe3O4 nanoparticles, forming uneven large particles and uneven particle distribution, which affects the magnetic and adsorption properties of the material. Too high a pH value may also cause excessive adsorption of hydroxides or other by-products on the surface of Fe3O4 particles, affecting the stability and dispersibility of the particles.
[0047] When the reaction temperature is lower than 85°C, the reaction rate of iron ions slows down and the formation process of Fe3O4 is inhibited, resulting in insufficient number of magnetic nanoparticles and poor magnetic performance. Under low temperature conditions, the Fe3O4 particles generated may have low crystallinity, affecting the stability and magnetic properties of the particles, and ultimately leading to insufficient magnetism of the GO@PAA@Fe3O4 composite material.
[0048] When the reaction temperature exceeds 95°C, the reaction rate of the iron salt accelerates, resulting in rapid growth and excessive aggregation of Fe3O4 particles, forming larger particles, reducing the specific surface area and adsorption performance of the material; under high temperature conditions, the PAA or GO structure in the system may be thermally damaged, resulting in decreased material stability or structural destruction, affecting the material's magnetic properties and other functional properties.
[0049] The reason why the present invention limits the reaction time to 3.5-5.5h is as follows: when the reaction time is insufficient, the iron ions cannot fully react, resulting in an insufficient number of Fe3O4 nanoparticles, weak magnetism, and the presence of incompletely reacted iron salt residues, which affects the purity and performance of the material. The Fe3O4 particles generated have low crystallinity, resulting in decreased stability and magnetic properties, affecting the actual application effect of the GO@PAA@Fe3O4 composite material.
[0050] Too long a reaction time will cause the Fe3O4 nanoparticles to continue to grow, resulting in excessive particle size, which in turn reduces its specific surface area and affects the magnetic and adsorption properties of the material. Long-term high-temperature reaction may also cause the structure of GO or PAA to degrade or polymerize, destroying the stability of the material and reducing the dispersion and functionality of the material.
[0051] In a preferred embodiment of the present invention, in step 3, the acidic acetone solution is a mixture of acetone and formic acid in a volume ratio of 199:1; and the activation is specifically ultrasonic activation at 25-45°C for 10-20 min.
[0052] The purpose of the present invention using an acidic acetone solution for activation is to enhance the exposure and modification of surface functional groups of graphene oxide composite nanomaterials (GO@PAA@Fe3O4) through an acidic environment, especially the exposure of active groups such as carboxyl and hydroxyl groups, thereby improving the reactivity and adsorption performance of the material. This acidic solution can effectively remove impurities or incompletely reacted substances on the surface of the material, while optimizing its surface structure to give it a higher surface energy, further enhancing the adsorption capacity for target molecules. In addition, the acidic environment can promote the dispersibility of the material, avoid particle agglomeration, and ensure the uniform distribution of the material during the adsorption process.
[0053] In the present invention, the activation temperature is limited to 25-45°C for the following reasons: When the temperature is lower than 25°C, the activation effect of the acidic acetone solution is weakened. Lower temperatures will lead to insufficient exposure of functional groups on the surface of the material, insufficient activation, and possible residual impurities, which will affect the subsequent adsorption performance. The dispersibility of the material may also be affected, and the particles are more likely to agglomerate, which will lead to a decrease in adsorption efficiency; when the temperature exceeds 45°C, the volatility of acetone and formic acid increases, and the stability of the solution deteriorates, which may cause excessive reaction or structural damage on the surface of the material, reducing the stability of the material. Excessively high temperatures may also cause the amide bond between PAA (polypropylene amine) and GO (graphene oxide) to be destroyed, affecting the structural integrity and adsorption function of the composite material.
[0054] In the present invention, if the activation time is insufficient, the surface activation effect of the material is insufficient, and the surface functional groups are not fully exposed, which may lead to a decrease in adsorption capacity. The surface impurities or unreacted products of the material cannot be completely removed, affecting its ability to bind to the target molecules (such as indole-3-acetic acid, indole-3-propionic acid) in the subsequent adsorption process; too long an activation time may cause over-reaction or destruction of the functional groups on the surface of the material, especially the active groups on the surface of the material may be over-modified or chemically damaged, resulting in a decrease in adsorption performance.
[0055] A second aspect of the present invention provides a graphene oxide composite nanomaterial prepared according to the above-mentioned preparation method.
[0056] The third aspect of the present invention provides an application of the above-mentioned graphene oxide composite nanomaterial in the adsorption of indole-3-acetic acid and indole-3-propionic acid.
[0057] The present invention evaluates the adsorption performance of GO@PAA@Fe3O4 on indole-3-acetic acid (IAA) and indole-3-propionic acid (IPA) through adsorption kinetics and adsorption isotherm experiments. The specific evaluation method is as follows:
[0058] Prepare a mixed standard solution of IAA and IPA, then add GO@PAA@Fe3O4, shake and adsorb at 25-45°C for different time, adsorb the GO@PAA@Fe3O4 composite material with a magnet, take the supernatant, filter the membrane and perform HPLC analysis; prepare a mixed standard solution of IAA and IPA with different concentrations, then add GO@PAA@Fe3O4 composite material, shake and adsorb at 25-45°C until saturation, take the supernatant, filter the membrane and perform HPLC analysis;
[0059] Preferably, the addition amount of the GO@PAA@Fe3O4 composite material is 0.3 g / L;
[0060] Preferably, the different adsorption times are 0-240 min, and more than 15 time gradients are set;
[0061] Preferably, the mixed standard solutions of different concentrations are 5-200 mg / L, and more than 15 concentration gradients are set;
[0062] Preferably, the HPLC conditions are: the chromatographic column uses Agilent ZORBAX Eclipse Plus C18 (5μm, 4.6mm×250mm); the column temperature is 30°C; the flow rate is 0.5mL / min; the injection volume is 10μL; the mobile phase contains 2% formic acid solution (phase A) and acetonitrile (phase B); the gradient elution program is: 0-5min, 20% B; 5-10min, 20%-70% B; 10-20min, 70%-80% B; 20-21min, 80%-20% B, 21-25min, 20% B. The detection wavelength is 280nm, and the absorption wavelength of the chromatographic peak is in the range of 400-600nm.
[0063] The technical solutions described in the present invention, unless otherwise specified, are all conventional solutions in the art, and the reagents or raw materials used, unless otherwise specified, are purchased from commercial channels or have been disclosed.
[0064] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0065] Example 1
[0066] Preparation and activation of graphene oxide composite nanomaterials (GO@PAA@Fe3O4):
[0067] like Figure 1 As shown in Figure 2, the synthetic route of GO@PAA@Fe3O4 mainly includes the self-assembly of polyacrylamine (PAA) (A) and the preparation of magnetic GO@PAA (B).
[0068] In the first step of material synthesis, the -COOH group on GO was activated and coupled with the -NH2 of PAA to form an amide bond according to the EDC-NHS coupling reaction (see Figure 1A). The specific steps are as follows: PAA is ultrasonically dispersed in 30.0 mL, 0.1 M potassium phosphate buffer (pH = 7.4) to a concentration of 25 mg / mL to obtain a PAA solution. In addition, 50 mg of GO powder is fully dissolved in 10 mL of MES buffer solution (50.0 mM, pH = 6.0), and 16 mg / mL EDC (Chinese name: N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide) and 24 mg / mL NHS (Chinese name: N-hydroxysuccinimide) are added in sequence, and the mixed solution is slowly shaken in a shaker at 37°C for 15 minutes for activation. After activation, the GO-EDC-NHS system is centrifuged at 3778.8×g for 10 minutes, and repeatedly rinsed with MES solution 3 times to remove the unreacted EDC and NHS solution. GO-EDC-NHS is slowly added to the PAA solution and reacted for 4 hours under mechanical stirring at room temperature. Finally, the supernatant was removed by centrifugation at 3778.8×g, and the reaction product was repeatedly washed with ultrapure water until the washing solution was neutral. The product was dried in a freeze dryer at -50°C for 24 hours to obtain GO@PAA powder.
[0069] The preparation of magnetic GO@PAA mainly adopts the co-precipitation method of iron salt and GO@PAA (see Figure 1 B). Specifically, 0.1988g FeCl2·4H2O and 0.5406g FeCl3·6H2O were dissolved in 20mL of 0.4mol / L HCl solution to obtain FeCl3 / FeCl2 / HCl solution. In addition, 0.06g of GO@PAA powder was ultrasonically dispersed in 20mL of ultrapure water at 35°C for 15min to obtain GO@PAA solution. The uniformly dispersed GO@PAA solution was added dropwise to the FeCl3 / FeCl2 / HCl solution and magnetically stirred for 1h at room temperature. After stirring, 160mL of 1.25M ammonia solution was added dropwise at a rate of 10 drops / min (so that the reaction system was in an alkaline condition of pH 10-12.0) and reacted at 90°C for 4h. Finally, the reaction product was adsorbed by a magnet and repeatedly washed with ultrapure water until the washing liquid was neutral. The washed product was dried in an oven at 60 °C overnight and labeled as N-GO@PAA@Fe3O4 (N-GPF).
[0070] After the N-GO@PAA@Fe3O4 composite material is synthesized, 0.5% acidic acetone (acetone / formic acid = 199:1, v / v) is added to activate the above material. The specific steps are as follows: Take 15 mg of N-GO@PAA@Fe3O4 composite material in a 10 mL centrifuge tube, add 5 mL of acidic acetone solution with a volume concentration of 0.5%, and ultrasonically activate it at 35°C for 15 minutes. Then, the above reaction product is adsorbed by a magnet and repeatedly washed with acetonitrile and ultrapure water in turn until the washing liquid is neutral. The washed product is placed in a 60°C oven and dried for 6 hours to remove all solvents. Finally, the graphene oxide composite nanomaterial GO@PAA@Fe3O4 is obtained.
[0071] In the present invention, TEM and SEM are used to characterize the morphology of GO, GO@PAA and GO@PAA@Fe3O4. Through TEM analysis, it can be clearly seen that ( Figure 2 A) GO presents a transparent lamellar structure with a rough surface and typical wrinkles. Compared with GO, GO@PAA( Figure 2 In B) the same lamellar structure is also shown. Figure 2 As shown in Figure C, Fe3O4 is gray, regular spherical, with an average particle size of about 10-15nm, and is successfully deposited on the GO@PAA sheet structure. SEM images of GO, GO@PAA, and GO@PAA@Fe3O4 are shown in Figure 3. Figure 2 DF. Compared with the SEM images of GO, the surface of GO@PAA has more wrinkles. Figure 2 As shown in Figure 5(F), since the surface of GO@PAA@Fe3O4 is uniformly covered with single or partially aggregated Fe3O4 nanoparticles, the surface of GO@PAA@Fe3O4 is rougher than that of GO@PAA, which is consistent with the results of TEM analysis.
[0072] In order to verify the successful synthesis of GO@PAA@Fe3O4 and investigate the chemical structure changes after GO functionalization, the present invention uses FTIR to characterize GO, GO@PAA and GO@PAA@Fe3O4. The spectra are shown in the following figure. Figure 3 shown. Figure 4 This is the XPS full scan spectrum of GO@PAA@Fe3O4. Figure 5 We can clearly see that there are characteristic absorptions at 285eV, 530eV, 398eV and 711eV binding energies, which are attributed to C1s, O1s, N1s and Fe 2p, respectively. In the high-resolution spectrum of C1s, we analyzed and obtained three characteristic peaks at 284.9eV, 286.5eV and 288.6eV, which correspond to the C=C, C-OH and COC and C=O functional group structures (see Figure 5 A); and in the high-resolution spectrum of O1s, there are four characteristic peaks, corresponding to C=O (532.9 eV), CO (531.4 eV), -OH (529.9 eV) and Fe-O (530.4 eV) ( Figure 5 (B) Figure 6 As shown, when the pH is 3.07, the isoelectric point (PI) of GO is reached; compared with GO, the isoelectric point of GO@PAA@Fe3O4 is higher (PI=5.35). In the present invention, GO@PAA@Fe3O4 has good stability, and the zeta potential is in the range of 26.5mV to -22.2mV. The present invention uses thermogravimetric analysis to investigate the thermal stability of GO, GO@PAA and GO@PAA@Fe3O4, respectively. In the specific experiment, the sample to be tested was protected with N2, and then its mass change from room temperature to 1000°C was investigated at a heating rate of 10°C / min. The test results are shown as follows. Figure 7 As shown. Compared with GO or GO@PAA, GO@PAA@Fe3O4 has higher thermal stability. At 27°C, VSM analysis was used to investigate the magnetic properties of GO@PAA@Fe3O4. Figure 8 As shown, the hysteresis loop curve of GO@PAA@Fe3O4 nanoparticles is "S"-shaped and passes through the origin. The remanence and coercive force are small and can be ignored, indicating that the material has good superparamagnetism.
[0073] In summary, these results indicate that GO@PAA@Fe3O4 was successfully synthesized and possessed advantages such as good adsorption sites, thermal stability, and superparamagnetism.
[0074] Example 2
[0075] Preparation of simulated wine samples: Use a certain volume of anhydrous ethanol (chromatographic grade) and ultrapure water to prepare an ethanol-water solution with a volume fraction of 15%, and use 4 mol / L HCl solution to adjust the pH to 4.0 as a simulated wine sample, and store it in a refrigerator at 4°C for use.
[0076] Preparation of mixed standard solution: Take standard samples of indole-3-acetic acid (2800 mg / L) and indole-3-propionic acid (3090 mg / L) respectively and place them in 10 mL volumetric flasks, make up to volume with ethanol solution to prepare a mixed standard stock solution with a mass fraction of 500 mg / L, and store it in a refrigerator at -4°C for use.
[0077] Take 5mL of the prepared simulated wine sample in a 50mL conical flask, add 20μL of the mixed standard solution of IAA and IPA to make the concentration in the sample 20mg / L, and then add 15mg GO@PAA@Fe3O4 nanoparticles. Place the above conical flask in a constant temperature oscillator at 35℃ and shake at 180r / min for 0, 30s, 2.5min, 5min, 10min, 20min, 30min, 40min, 60min, 90min, 120min, 150min, 180min, 210min, 240min, then take out the conical flask, adsorb GO@PAA@Fe3O4 nanoparticles with a magnet, take the upper clear liquid, filter it through a 0.22μm filter membrane, and perform HPLC analysis. The adsorption amount of IAA and IPA is calculated according to the following formula (1). Set up 3 parallel tests for each test time.
[0078] Q t =(C0-C t )V / m(1)
[0079] Q in the formula t is the adsorption amount of IAA or IPA by GO@PAA@Fe3O4 at time t (mg / g); C0 and C t are the initial concentration of the test compound and the concentration at time t (mg / L); V is the volume of the test sample (mL); m is the mass of GO@PAA@Fe3O4 (mg).
[0080] HPLC procedure: The chromatographic column used was Agilent ZORBAX Eclipse Plus C18 (5 μm, 4.6 mm×250 mm); the column temperature was 30° C.; the flow rate was 0.5 mL / min; the injection volume was 10 μL; the mobile phase contained 2% formic acid solution (phase A) and acetonitrile (phase B); the gradient elution program was: 0-5 min, 20% B; 5-10 min, 20%-70% B; 10-20 min, 70%-80% B; 20-21 min, 80%-20% B, 21-25 min, 20% B. The detection wavelength was 280 nm, and the absorption wavelength of the chromatographic peak was in the range of 400-600 nm.
[0081] In order to investigate the adsorption rate of IAA and IPA in the sample and the adsorption equilibrium time of GO@PAA@Fe3O4, an adsorption kinetic experiment was carried out in the present invention. Fig. 9 As shown in a in A and a in B, most of IAA and IPA were rapidly adsorbed within 10 min, and then entered a relatively slow adsorption process until adsorption equilibrium was reached. Finally, when IAA and IPA reached adsorption equilibrium, their adsorption amounts were 3.69 mg / g and 3.59 mg / g, respectively.
[0082] In order to further clarify the adsorption mechanism of GO@PAA@Fe3O4 on IAA and IPA, the pseudo-first-order kinetic model and pseudo-second-order kinetic model were used to fit the experimental data of IAA and IPA adsorption at different adsorption times. The calculation formulas of the pseudo-first-order kinetic model (2) and pseudo-second-order kinetic model (3) are as follows:
[0083] ln(Q e -Q t )=-k1t+ln Q e (2)
[0084]
[0085] Q in the formula t and Q e (mg / g) are the adsorption amounts of IAA and IPA on GO@PAA@Fe3O4 at t(min) and equilibrium state, respectively; k1(1 / min) and k2(g·(mg·min) -1 ) are the adsorption rate constants of pseudo-first-order kinetic model and pseudo-second-order kinetic model respectively. Fig. 9 (In the figure, Experimental data in a and b represent the adsorption kinetic experimental data obtained by detection; Pseudo-first-order model for IAA represents the fitting curve of the pseudo-first-order kinetic model for IAA adsorbed by GO@PAA@Fe3O4; Pseudo-second-order model for IAA represents the fitting curve of the pseudo-second-order kinetic model for IAA adsorbed by GO@PAA@Fe3O4; Experimental in c and d represent the adsorption isotherm experimental data obtained by detection; Pseudo-first-prdermodel for IPA represents the fitting curve of the pseudo-first-order kinetic model for IPA adsorbed by GO@PAA@Fe3O4; Pseudo-second-order model for IPA represents the fitting curve of the pseudo-second-order kinetic model for IPA adsorbed by GO@PAA@Fe3O4) The data in b,c in A and b,c in B show that the linear correlation coefficient (R 2 =0.9999, 0.9999) were significantly higher than the linear correlation coefficient (R 2 =0.8269, 0.9030), and the Q of IAA and IPA were calculated by pseudo-second-order kinetic model. eThe values (3.71 mg / g and 3.62 mg / g) are very close to the experimental values (3.69 mg / g and 3.59 mg / g). In summary, the pseudo-second-order kinetic model can better describe the adsorption of IAA and IPA in the sample by GO@PAA@Fe3O4, and further illustrates that GO@PAA@Fe3O4 mainly extracts IAA and IPA in the sample through surface adsorption.
[0086] Example 3
[0087] Take 5mL of the simulated wine sample prepared in Example 2 in a 50mL conical flask, add 20μL of the mixed standard solution of IAA and IPA respectively, so that the concentration in the sample is in the range of 5-200mg / L, and then add 15mg GO@PAA@Fe3O4 nanoparticles. Place the above conical flask in a constant temperature oscillator at 35°C and shake at 180r / min for a sufficient adsorption time, then take out the conical flask, adsorb GO@PAA@Fe3O4 nanoparticles with a magnet, take the upper clear liquid, filter it through a 0.22μm filter membrane, perform HPLC analysis, and calculate the adsorption amount of IAA and IPA. Set up 3 parallel tests at each test concentration.
[0088] HPLC procedure: The chromatographic column used was Agilent ZORBAX Eclipse Plus C18 (5 μm, 4.6 mm×250 mm); the column temperature was 30° C.; the flow rate was 0.5 mL / min; the injection volume was 10 μL; the mobile phase contained 2% formic acid solution (phase A) and acetonitrile (phase B); the gradient elution program was: 0-5 min, 20% B; 5-10 min, 20%-70% B; 10-20 min, 70%-80% B; 20-21 min, 80%-20% B, 21-25 min, 20% B. The detection wavelength was 280 nm, and the absorption wavelength of the chromatographic peak was in the range of 400-600 nm.
[0089] In the present invention, the adsorption isotherms of GO@PAA@Fe3O4 for IAA and IPA were investigated. The adsorption of IAA and IPA increased with the increase of concentration until saturation was reached. In order to further investigate the interaction between GO@PAA@Fe3O4 and IAA and IPA, we used the Langmuir and Freundlich isotherm adsorption models to fit the above experimental data (see Fig.10In the figure, Experimental data in A and B represent the experimental data obtained by the adsorption isotherm detection of IAA by GO@PAA@Fe3O4; Experimental data in C and D represent the experimental data obtained by the adsorption isotherm detection of IPA by GO@PAA@Fe3O4; Freundlich model of IAA and Freundlich model of IPA represent the Freundlich model fitting curves of IAA and IPA adsorbed by GO@PAA@Fe3O4, respectively).
[0090] The Langmuir isotherm adsorption model is usually used to describe the monolayer adsorption on a homogeneous surface. That is, it is assumed that all adsorption sites on the adsorbent surface have the same adsorption capacity. Therefore, when the adsorbate binds to the adsorption site, there will be no interaction between them. In addition, compared with the Langmuir isotherm adsorption model, the Freundlich isotherm adsorption model is used to describe the multilayer adsorption on a heterogeneous surface, and the adsorption amount will increase indefinitely with the increase of the adsorbate concentration. The calculation formulas of the Langmuir isotherm adsorption model (4) and the Freundlich isotherm adsorption model (5) are as follows:
[0091]
[0092] Q in the formula max (mg / g) is the maximum adsorption capacity of GO@PAA@Fe3O4 for IAA or IPA; K L (L / mg) is the equilibrium constant in the Langmuir isotherm adsorption model; K f ((mg / g)·(L / mg) 1 / n ) and 1 / n are Freundlich isotherm constants, which are used to describe the adsorption amount and adsorption intensity, respectively.
[0093] according to Fig.10 The data show that the linear correlation coefficient (R 2 =0.9992, 0.9919) are the highest, and the Q values of IAA and IPA calculated by this model are maxThe values (14.3 mg / g and 14.0 mg / g) are closest to the experimental values. Therefore, the above results show that the adsorption isotherms of GO@PAA@Fe3O4 for IAA and IPA are more consistent with the Langmuir isotherm adsorption model. In summary, the adsorption isotherms of GO@PAA@Fe3O4 for IAA and IPA are consistent with the Langmuir isotherm adsorption model; at the same time, the above adsorption process is a monolayer adsorption on a homogeneous surface, and the adsorption sites provided by GO@PAA@Fe3O4 have the same adsorption energy and the same affinity for IAA and IPA. Finally, at 35°C, the maximum adsorption amounts of GO@PAA@Fe3O4 for IAA and IPA were 14.3 mg / g and 14.0 mg / g, respectively.
[0094] Comparative Example 1
[0095] 1) First, 2.4 g FeCl3·6H2O, 2.4 g CH3COONa, 30 mL ethylene glycol and 0.54 g PEG 2000 surfactant were added to the reactor respectively, and then 0.25 g GO was added and ultrasonically dispersed for 5 min. After reacting at 200 °C for 12 h, the reactor was cooled to room temperature. Then, the product in the reactor was poured into a beaker, and an external magnet was used to make the black nanomaterial in the beaker to obtain magnetic graphene oxide Fe3O4@GO.
[0096] 2) 100 mg Fe3O4@GO, 5 mL acrylic acid (AA, purity> 99%), and 45 mL (concentration of 2 mg / mL) of FeSO4 aqueous solution were added to the test tube, ultrasonically dispersed evenly (ultrasonic power 80 W, time 5 min), and sealed after passing high-purity N2 gas for 15 min. The sealed test tube was irradiated with 60Coγ-rays at a dose rate of 20 Gy / min and a dose of 20 kGy.
[0097] 3) The irradiated product was transferred to a beaker, and the black magnetic material and the supernatant were separated by an external magnet, and then ultrasonically washed alternately with distilled water and ethanol for multiple times. After washing, the product was dried in a vacuum oven at 60°C to obtain a magnetic graphene oxide composite material Fe3O4@GO-g-(PAA).
[0098] The Fe3O4@GO-g-(PAA) prepared in this comparative example was subjected to the same effect verification as in Example 3. The results showed that the maximum adsorption amounts of IAA and IPA by the Fe3O4@GO-g-(PAA) prepared in this comparative example were 3.15 mg / g and 4.22 mg / g, respectively.
[0099] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a graphene oxide composite nanomaterial, characterized in that: The following steps are involved: Step 1: According to the EDC-NHS coupling reaction, the -COOH group on GO is activated and coupled with the -NH2 of PAA to form an amide bond to obtain GO@PAA; Step 2, preparing magnetic GO@PAA by co-precipitation of iron salt and GO@PAA; Step 3, using an acidic acetone solution to activate the magnetic GO@PAA and wash it to obtain a graphene oxide composite nanomaterial.
2. The method for preparing the graphene oxide composite nanomaterial according to claim 1, wherein: In step 1, PAA is dissolved in buffer 1 to obtain a PAA solution; EDC and NHS were sequentially added into buffer 2 containing GO powder for activation to obtain GO-EDC-NHS; The PAA solution and the GO-EDC-NHS are mixed and stirred to react to obtain GO@PAA.
3. The method for preparing the graphene oxide composite nanomaterial according to claim 2, wherein: The mass ratio of the GO to the PAA is 1:
15.
4. The method for preparing the graphene oxide composite nanomaterial according to claim 1, wherein: In step 2, after the GO@PAA is dispersed in water, it is added to an acidic solution containing iron salt and mixed evenly, and then an ammonia solution is added to react to obtain magnetic GO@PAA.
5. The method for preparing the graphene oxide composite nanomaterial according to claim 4, characterized in that: The iron salt is a mixture of a divalent iron salt and a trivalent iron salt; the molar ratio of the divalent iron salt to the trivalent iron salt is 1:2; and the acidic solution is a 0.2-0.6 mol / L HCl solution.
6. The method for preparing the graphene oxide composite nanomaterial according to claim 4, characterized in that: The mass ratio of the iron salt to the GO@PAA is 12-13:
1.
7. The method for preparing the graphene oxide composite nanomaterial according to claim 4, characterized in that: The reaction is specifically carried out at a pH of 10-12 and a temperature of 85-95° C. for 3.5-5.5 hours.
8. The method for preparing the graphene oxide composite nanomaterial according to claim 1, characterized in that: In step 3, the acidic acetone solution is a mixture of acetone and formic acid in a volume ratio of 199:1; and the activation is specifically ultrasonic activation at 25-45° C. for 10-20 min.
9. The graphene oxide composite nanomaterial prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the graphene oxide composite nanomaterial according to claim 9 in the adsorption of indole-3-acetic acid and indole-3-propionic acid.
Citation Information
Patent Citations
Magnetic graphene oxide composite material for removing tetracycline hydrochloride in aqueous solution and preparation method thereof
CN109107531A
Magnetic graphene oxide composite material as well as preparation method and application thereof
CN111318255A
Nano composite material and application thereof in detection of ester substances in wine
CN113219116A
Magnetic composite having multi nano-layers on magnetic nanoparticle surface and manufacturing method thereof