Catalyst for synthesizing n-butyronitrile, preparation method of catalyst and synthesis method of n-butyronitrile

By using a special catalyst to carry out ammonia dehydration reaction with n-butyric acid at high temperature, the problem of difficulty in separation of n-butyric nitrile and n-butanol was successfully solved, and the synthesis of high-purity n-butyric nitrile was achieved, with a simple process and low cost.

CN119075964APending Publication Date: 2024-12-06BEIJING FLEMING TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411209714.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing synthesis methods of n-butyrogen nitrile, the difficulty in isolating n-butyrogen and n-butanol leads to low purity and lacks effective solutions.

Method used

A new catalyst is used to prepare the catalyst by mixing alumina powder, binder and water in a specific proportion, kneading, extruding, drying and calcining, and the catalyst is used to be with n-butyric acid at 380-420°C. Ammonia dehydration reaction was carried out, and high-purity n-nitrile separation was obtained by stratification and distillation.

Benefits of technology

The synthesis of n-butyrgan nitrile with high conversion and high purity has been achieved, which solves the problem of difficult separation of n-butyrgan and n-butanol. The process is simple and feasible, the catalyst has high selectivity and stability, and the production cost is low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020024280000071
    Figure BDA0005020024280000071
  • Figure BDA0005020024280000081
    Figure BDA0005020024280000081
Patent Text Reader

Abstract

The invention relates to the technical field of organic synthesis of n-butyronitrile, in particular to a catalyst for synthesizing n-butyronitrile, a preparation method of the catalyst and a synthesis method of n-butyronitrile. The catalyst for synthesizing n-butyronitrile comprises the following components in parts by weight: 300-500 parts of powder; 110 to 220 parts of a binder; 100 to 300 parts of water; the powder comprises any one of alumina powder, silicon dioxide powder, titanium dioxide and a molecular sieve; the binder comprises any one or more of alumina sol, silica sol, nitric acid and high clay. The catalyst provided by the invention has the advantages of high conversion rate, high selectivity, good stability, low production cost and the like. According to the present invention, the synthesis reaction of n-butyronitrile is performed by using the catalyst, which is a new reaction mode, and is different from the traditional mode of producing n-butyronitrile by using n-butanol ammoniation, the problem of difficult separation of n-butyronitrile and n-butanol does not exist by using the synthesis method provided by the present invention, and the process is simple, convenient and feasible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of organic synthesis of n-butyronitrile, and in particular to a catalyst for synthesizing n-butyronitrile and a preparation method thereof, and a method for synthesizing n-butyronitrile. Background Art

[0002] Butyronitrile is an important chemical product and is widely used in the chemical industry. It can be used as an intermediate in drug synthesis and as an additive for industrial products.

[0003] At present, n-butyronitrile is mainly synthesized by catalytic amination of n-butanol or n-butyraldehyde. In the product recovery of this synthesis method, there is a problem of difficulty in separating n-butyronitrile and n-butanol, so the purity of the obtained n-butyronitrile is low. However, there is no better solution for the problem of difficulty in separating n-butyronitrile and n-butanol.

[0004] Based on the above, it is necessary to seek a new synthesis method for n-butyronitrile or to work on solving the problem of the difficulty in separating n-butyronitrile and n-butanol. Summary of the invention

[0005] The present application provides a catalyst for synthesizing n-butyronitrile and a preparation method thereof, and a method for synthesizing n-butyronitrile.

[0006] The catalyst for synthesizing n-butyronitrile provided in the present application has the advantages of high conversion rate, high selectivity, good stability, low production cost, etc. The present application uses the above catalyst to carry out the synthesis reaction of n-butyronitrile, which is a new reaction mode. Different from the traditional method of producing n-butyronitrile by ammoniation of n-butanol, the synthetic method of the present application does not have the problem of difficulty in separating n-butyronitrile and n-butanol, and the process is simpler and more feasible.

[0007] By using the catalyst for synthesizing n-butyronitrile provided in the present application, n-butyric acid is used as a raw material to carry out a catalytic amination and dehydration reaction to prepare n-butyronitrile, wherein the conversion rate of n-butyric acid can reach more than 99%, the mass yield is about 72%, and the molar yield can reach 92%.

[0008] The product solution obtained after the reaction is layered, the upper layer is a normal butyronitrile solution, and the lower layer is an ammonia and water solution. After layering and separation, the content of normal butyronitrile in the upper layer solution is more than 93%, and it also contains a small amount of ammonia and water, which is relatively easy to separate by distillation. After distillation and separation, more than 99.8% of normal butyronitrile can be obtained. Therefore, the synthesis method of the present application can obtain high-purity normal butyronitrile through a simple process.

[0009] In a first aspect, the present application provides a catalyst for synthesizing n-butyronitrile, using the following technical solution:

[0010] A catalyst for synthesizing n-butyronitrile, the catalyst comprising the following components in parts by weight: 300-500 parts of powder; 100-220 parts of binder; 100-300 parts of water;

[0011] The powder includes any one of alumina powder, silica powder, titanium dioxide, and molecular sieve;

[0012] The binder includes any one or more of aluminum sol, silica sol, nitric acid, and high clay.

[0013] Optionally, the weight portion of the powder is 350-450 parts.

[0014] In a specific embodiment, the weight parts of the powder are 300 parts, 350 parts, 400 parts, 450 parts or 500 parts.

[0015] In some specific embodiments, the weight proportions of the powder are 300-350 parts, 300-400 parts, 300-450 parts, 350-400 parts, 350-450 parts, 350-500 parts, 400-450 parts, 400-500 parts, 450-500 parts.

[0016] Optionally, the powder is alumina powder.

[0017] Optionally, the powder is silicon dioxide powder.

[0018] Optionally, the powder is titanium dioxide.

[0019] Optionally, the powder is a molecular sieve.

[0020] Optionally, the weight portion of the binder is 120-200 parts.

[0021] In a specific embodiment, the weight proportion of the binder is 100 parts, 120 parts, 160 parts, 200 parts or 220 parts.

[0022] In some specific embodiments, the weight proportion of the binder is 100-120 parts, 100-160 parts, 100-200 parts, 120-160 parts, 120-200 parts, 120-220 parts, 160-200 parts, 160-220 parts, 200-220 parts.

[0023] Optionally, the binder includes kaolin and any one of aluminum sol, silica sol and nitric acid.

[0024] Optionally, the binder is aluminum sol and high clay.

[0025] Optionally, the binder is silica sol and high clay.

[0026] Optionally, the binder is nitric acid and high clay.

[0027] Optionally, the binder is aluminum sol, silica sol and high clay.

[0028] Optionally, the binder is aluminum sol, nitric acid and high clay.

[0029] Optionally, the binder is silica sol, nitric acid and high clay.

[0030] Optionally, the binder is aluminum sol, silica sol, nitric acid and high clay.

[0031] Optionally, the weight portion of the water is 150-250 parts.

[0032] In a specific embodiment, the weight parts of water are 100 parts, 150 parts, 200 parts, 250 parts or 300 parts.

[0033] In some specific embodiments, the weight parts of water are 100-150 parts, 100-200 parts, 100-250 parts, 150-200 parts, 150-250 parts, 150-300 parts, 200-250 parts, 200-300 parts, 250-300 parts.

[0034] In a second aspect, the present application provides a method for preparing the above-mentioned catalyst, using the following technical solution:

[0035] A method for preparing a catalyst comprises the following steps: uniformly mixing the powder and the binder and then adding the water, and after uniform mixing, kneading, extruding, drying and calcining are sequentially performed to obtain the catalyst.

[0036] Optionally, the preparation method specifically comprises the following steps:

[0037] (1) mixing the powder and the binder uniformly according to the ratio requirement, adding the water, and kneading the mixed powder and the binder by a kneader to obtain a kneaded material; the kneader has a rotation speed of 30-70 r / min, and the kneading time is 6-10 h;

[0038] (2) placing the kneaded material into an extruder for extrusion to obtain extruded strips;

[0039] (3) drying the extruded sample to obtain a dried sample; the drying temperature is 120-150° C., and the drying time is 4-12 h;

[0040] (4) calcining the dried sample at 500-700° C. for 3-10 hours to obtain the catalyst.

[0041] Optionally, the extruder is a hydraulic extruder;

[0042] Optionally, the die of the hydraulic extruder is a three-tooth type with a tooth pitch of 2.5 mm;

[0043] Optionally, the extrusion pressure of the hydraulic extruder is 6-10 MPa;

[0044] Optionally, the extruded sample strips are dried in a blast oven;

[0045] Optionally, the heating rate of the temperature of the dried sample strips for roasting is 1-2°C / min.

[0046] In a third aspect, the present application provides a method for synthesizing n-butyronitrile, which uses the above-mentioned catalyst.

[0047] Optionally, the synthesis method specifically includes the following steps: under the catalytic action of the catalyst, using n-butyric acid as a raw material, carrying out an ammonia dehydration reaction with ammonia at 380-420° C., and separating the product by layering and water to obtain the n-butyronitrile.

[0048] Optionally, the molar ratio of the ammonia gas to the n-butyric acid is (1-3): 1;

[0049] Optionally, the amination-dehydration reaction is carried out in a fixed bed reactor;

[0050] Optionally, the volume space velocity of the n-butyric acid is 0.2-0.5h -1 ;

[0051] Optionally, the purity of the n-butyronitrile is greater than 99.8%.

[0052] In summary, the present application includes at least one of the following beneficial technical effects:

[0053] The catalyst for synthesizing n-butyronitrile provided in the present application has the advantages of high conversion rate, high selectivity, good stability, low production cost, etc. The present application uses the above catalyst to carry out the synthesis reaction of n-butyronitrile, which is a new reaction mode. Different from the traditional method of producing n-butyronitrile by ammoniation of n-butanol, the synthetic method of the present application does not have the problem of difficulty in separating n-butyronitrile and n-butanol, and the process is simpler and more feasible.

[0054] By using the catalyst for synthesizing n-butyronitrile provided in the present application, n-butyric acid is used as a raw material to carry out a catalytic amination and dehydration reaction to prepare n-butyronitrile, wherein the conversion rate of n-butyric acid can reach more than 99%, the mass yield is about 72%, and the molar yield can reach 92%.

[0055] The product solution obtained after the reaction is layered, the upper layer is a normal butyronitrile solution, and the lower layer is an ammonia and water solution. After layering and separation, the content of normal butyronitrile in the upper layer solution is more than 93%, and it also contains a small amount of ammonia and water, which is relatively easy to separate by distillation. After distillation and separation, more than 99.8% of normal butyronitrile can be obtained. Therefore, the synthesis method of the present application can obtain high-purity normal butyronitrile through a simple process. DETAILED DESCRIPTION

[0056] Before describing the embodiments of the present application in detail, it should be understood that the terms used herein are only used for the purpose of describing specific embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by ordinary technicians in the field to which the terms belong.

[0057] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of this application, unless otherwise specified, the meaning of "plurality" is two or more.

[0058] The endpoints and any values ​​of the ranges disclosed in this application are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0059] In the present application, the terms "comprise" or "include" are open expressions, that is, including the contents specified in the present application but not excluding other contents.

[0060] The present application provides a catalyst for synthesizing n-butyronitrile. The catalyst comprises the following components in parts by weight: 300-500 parts of powder; 100-220 parts of binder; 100-300 parts of water; the powder comprises any one of alumina powder, silica powder, titanium dioxide, and molecular sieve; the binder comprises any one or more of alumina sol, silica sol, nitric acid, and high clay.

[0061] The present application provides a method for preparing the above catalyst, which specifically comprises the following steps: uniformly mixing the powder and the binder and then adding the water, and then kneading, extruding, drying and calcining in sequence after uniform mixing to obtain the catalyst.

[0062] Specifically, the preparation method comprises the following steps:

[0063] (1) After the powder and the binder are mixed uniformly according to the ratio requirements, water is added and the raw materials are kneaded with a kneader until the raw materials are uniform, have no color difference, and can be formed by hand kneading to obtain a kneaded material.

[0064] The rotating speed of the kneading machine is 30-70 r / min, and the kneading time is 6-10 h.

[0065] (2) The kneaded material is placed into an extruder for extrusion to obtain extruded strips.

[0066] The extruder can be a hydraulic extruder, the die of which is a three-tooth type with a pitch of 2.5 mm and an extrusion pressure of 6-10 MPa.

[0067] (3) Drying the extruded specimen to obtain a dried specimen.

[0068] The extruded sample strips can be dried in a blast oven at a temperature of 120-150° C. and for a time of 4-12 hours.

[0069] (4) The dried sample strips are calcined at 500-700°C for 3-10 hours to obtain a catalyst. The heating rate of the calcined temperature after drying is 1-2°C / min.

[0070] In addition, the present application also provides a method for synthesizing n-butyronitrile, wherein the above catalyst is used in the method.

[0071] The synthesis method uses a pilot molten salt fixed bed reactor. The reactor has a reaction tube diameter of 25 mm; 50 ml of inert porcelain balls are loaded at the bottom of the reaction tube; 1000-2000 ml of catalyst is loaded on the top of the porcelain balls, and the catalyst height is about 2-4 meters; 100 ml of inert porcelain balls are loaded on the top of the reaction tube. Before the reaction, the catalyst is loaded into the fixed bed reactor, and after the catalyst is loaded, it is purged and replaced with nitrogen and tested for leaks.

[0072] In a specific embodiment, the above-mentioned method for synthesizing n-butyronitrile specifically comprises the following steps: using n-butyric acid as a raw material, carrying out an ammonia dehydration reaction with ammonia gas at 380-420° C. under the catalytic action of the catalyst, separating the product by stratification and water, and obtaining n-butyronitrile. The purity of the obtained n-butyronitrile is greater than 99.8%.

[0073] The molar ratio of ammonia to n-butyric acid is (1-3): 1. The ammonia dehydration reaction is carried out in a fixed bed reactor, and the volume space velocity of n-butyric acid is 0.2-0.5h -1 .

[0074] In a specific embodiment, the synthesis method of the above-mentioned n-butyronitrile specifically comprises the following steps:

[0075] After replacing the system with nitrogen, ammonia is introduced at a rate of 1-5L / min; the molten salt temperature of the fixed bed reactor is increased to 380-420°C; the preheater temperature is increased to 200°C.

[0076] After the temperature and gas volume are stable, n-butyric acid is fed in with a feed pump at a feed rate of 5-10 ml / min; n-butyric acid and ammonia are preheated in a preheater and then fed into a fixed bed reactor for reaction. The reactor outlet is connected to a cooling tower to recover the product, and the material is discharged and sampled for testing once every 4 hours.

[0077] In order to make the purpose, technical scheme and advantages of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. The embodiments described below are exemplary and are only used to explain the present application, and cannot be interpreted as limiting the present application.

[0078] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0079] The powder is a commercially available nano-scale product with no other special requirements. The molecular sieve model is ZSM-5, with a silicon-aluminum ratio of 100. In the binder, the aluminum sol requires an aluminum content of 10-15%; the silica sol requires a silicon dioxide content of 35%; the nitric acid concentration is an analytical pure solution of 68%; there is no requirement for high clay.

[0080] The present application is further described in detail below in combination with preparation examples, embodiments and test results.

[0081] Preparation Example

[0082] Preparation Example 1

[0083] This preparation example provides a catalyst for synthesizing n-butyronitrile.

[0084] The preparation method of the above catalyst specifically comprises the following steps:

[0085] (1) As shown in Table 1, take the powder and mix it, continue to add the binder, stir for 30 minutes, then add water, and knead it with a kneader until it is uniform, has no color difference, and can be formed by hand kneading to obtain the kneaded material. The speed of the kneader is 50r / min, and the kneading time is 8h.

[0086] (2) The kneaded material is placed in a hydraulic extruder for extrusion to obtain extruded strips. The die is a three-tooth type with a tooth pitch of 2.5 mm and an extrusion pressure of 8 MPa.

[0087] (3) The extruded sample is placed in a porcelain plate and dried in a forced air oven at a temperature of 120°C for 8 hours to obtain a dried sample.

[0088] (4) The dried sample was placed in a muffle furnace and calcined at 600°C for 6 h at a heating rate of 2°C / min to obtain a catalyst.

[0089] Preparation Example 2-12

[0090] Preparation Examples 2-12 respectively provide a catalyst for synthesizing n-butyronitrile.

[0091] The difference between the preparation method of the above catalyst and Preparation Example 1 is that the specific types and amounts of the raw materials used are shown in Table 1. The rest are consistent with the operating steps of Preparation Example 1.

[0092] The differences between the above preparation examples 1-12 are as follows:

[0093] The difference between Preparation Examples 1-4 lies in the specific type of powder used in the raw materials.

[0094] The difference between Preparation Examples 5-8 lies in the specific type of powder used in the raw materials.

[0095] The difference between Preparation Examples 9-12 lies in the specific type of powder used in the raw materials.

[0096] The difference between Preparation Examples 1, 5 and 9 lies in the specific type of binder in the raw materials used.

[0097] The difference between Preparation Examples 2, 6 and 10 lies in the specific type of binder in the raw materials used.

[0098] The difference between Preparation Examples 3, 7 and 11 lies in the specific type of binder in the raw materials used.

[0099] The difference between Preparation Examples 4, 8 and 12 lies in the specific type of binder in the raw materials used.

[0100] Table 1 Specific types and amounts of each component in the catalyst provided in each preparation example

[0101]

[0102] Examples 1-12

[0103] Examples 1-12 provide a method for synthesizing n-acetonitrile respectively. The difference between the above examples is that the catalysts of Preparation Examples 1-12 are used to synthesize n-acetonitrile respectively.

[0104] The reactor used in the synthesis method is a pilot molten salt fixed bed reactor, and the reaction tube diameter of the reactor is 25 mm.

[0105] The synthesis method specifically comprises the following steps:

[0106] (1) Catalyst loading

[0107] The bottom of the reaction tube is filled with 50 ml of inert porcelain balls; the top of the porcelain balls is filled with 1000 ml of catalyst, and the catalyst height is about 2 meters; the top of the reaction tube is filled with 100 ml of inert porcelain balls. After the catalyst is filled, it is purged and replaced with nitrogen and tested for leaks.

[0108] (2) Reaction

[0109] The temperature of the reactor molten salt was raised to 400°C, the temperature of the preheater was raised to 200°C, and ammonia was introduced at a rate of 2 L / min.

[0110] After the temperature and gas volume are stable, n-butyric acid is fed in with a feed pump at a feed rate of 8 ml / min. After being preheated in a preheater, n-butyric acid and ammonia enter a fixed bed reactor for reaction. The molar ratio of ammonia to n-butyric acid is 2:1.

[0111] After the reaction stabilized, the material was discharged every 4 hours, and sampling was performed once. The weight of the raw material and the discharged material was recorded, and the samples were analyzed using an Agilent 7820 gas chromatograph TCD detector.

[0112] Test results

[0113] The products obtained by the synthesis method provided in the above embodiment are specifically shown in Table 2.

[0114] Table 2 Test results of each embodiment

[0115]

[0116] As shown in Table 1, by comparing the test results of Examples 1-4, it can be seen that when the powder in the n-butyronitrile catalyst is alumina powder, the binder is silica sol and high clay, the molar yield of the reaction is the highest; by comparing the test results of Examples 5-8, it can be seen that when the powder in the n-butyronitrile catalyst is molecular sieve, the binder is aluminum sol and high clay, the molar yield of the reaction is the highest; by comparing the test results of Examples 9-12, it can be seen that when the powder in the n-butyronitrile catalyst is molecular sieve, the binder is nitric acid and high clay, the molar yield of the reaction is the highest. At the same time, by comparing the test results of Examples 1, 8 and 12, it can be seen that when the powder in the n-butyronitrile catalyst is alumina powder, the binder is silica sol and high clay, the molar yield of the reaction is the highest.

[0117] From the above, it can be seen that there is a synergistic effect between the powder and the binder in the n-butyronitrile catalyst of the present application. When different powders and binders are selected for compounding, the molar yield of the reaction will have certain differences.

[0118] In addition, by comparing the test results of Examples 1, 5, and 9, it can be seen that when the powder in the n-butyronitrile catalyst is alumina powder, and the binder is silica sol and high clay, the molar yield of the reaction is the highest; by comparing the test results of Examples 2, 6, and 10, it can be seen that when the powder in the n-butyronitrile catalyst is alumina powder, and the binder is silica sol and high clay, the molar yield of the reaction is the highest; by comparing the test results of Examples 3, 7, and 11, it can be seen that when the powder in the n-butyronitrile catalyst is alumina powder, and the binder is silica sol and high clay, the molar yield of the reaction is the highest; by comparing the test results of Examples 4, 8, and 12, it can be seen that when the powder in the n-butyronitrile catalyst is alumina powder, and the binder is silica sol and high clay, the molar yield of the reaction is the highest.

[0119] From the above, it can be seen that in the n-butyronitrile catalyst of the present application, when the powder in the n-butyronitrile catalyst is alumina powder and the binder is silica sol and high clay, the molar yield of the reaction is optimal.

[0120] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A catalyst for synthesizing n-butyronitrile, characterized in that The catalyst comprises the following components in parts by weight: 300-500 parts of powder; 100-220 parts of binder; 100-300 parts of water; The powder includes any one of alumina powder, silica powder, titanium dioxide, and molecular sieve; The binder includes any one or more of aluminum sol, silica sol, nitric acid, and high clay.

2. The catalyst according to claim 1, characterized in that The weight portion of the powder is 350-450 parts.

3. The catalyst according to claim 1, characterized in that The weight portion of the binder is 120-200 parts.

4. The catalyst according to claim 1, characterized in that The binder includes kaolin and any one of aluminum sol, silica sol and nitric acid.

5. A method for preparing the catalyst according to any one of claims 1 to 4, characterized in that: The preparation method specifically comprises the following steps: mixing the powder and the binder uniformly and then adding the water, and after mixing, kneading, extruding, drying and calcining are performed in sequence to obtain the catalyst.

6. The preparation method according to claim 5, characterized in that: The preparation method specifically comprises the following steps: (1) Mixing the powder and the binder evenly according to the ratio requirement, adding the water, and kneading the mixture using a kneader to obtain a kneaded material; the speed of the kneader is 30-70 r / min, and the kneading time is 6-10 h; (2) placing the kneaded material into an extruder for extrusion to obtain extruded strips; (3) drying the extruded sample strips to obtain dried sample strips; the drying temperature is 120-150° C., and the drying time is 4-12 hours; (4) calcining the dried sample at 500-700° C. for 3-10 hours to obtain the catalyst.

7. The preparation method according to claim 6, characterized in that: The extruder is a hydraulic extruder; Optionally, the die of the hydraulic extruder is a three-tooth type with a tooth pitch of 2.5 mm; Optionally, the extrusion pressure of the hydraulic extruder is 6-10 MPa; Optionally, the extruded sample strips are dried in a blast oven; Optionally, the heating rate of the temperature of the dried sample strips for roasting is 1-2°C / min.

8. A method for synthesizing n-butyronitrile, characterized in that: The synthesis method uses the catalyst described in any one of claims 1 to 4.

9. The synthesis method according to claim 8, characterized in that The synthesis method specifically comprises the following steps: Under the catalytic action of the catalyst, n-butyric acid is used as a raw material and subjected to an ammoniation dehydration reaction with ammonia at 380-420° C. The product is subjected to layering treatment and separated from water to obtain the n-butyronitrile.

10. The synthesis method according to claim 9, characterized in that The molar ratio of the ammonia gas to the n-butyric acid is (1-3): 1; Optionally, the amination-dehydration reaction is carried out in a fixed bed reactor; Optionally, the volume space velocity of the n-butyric acid is 0.2-0.5h -1 ; Optionally, the purity of n-butyronitrile is greater than 99.8%.