MOF-zirconium-based noble metal catalyst for catalytic oxidation of VOCs as well as preparation method and application of MOF-zirconium-based noble metal catalyst

Through the preparation of MOF-zirconium-based precious metal catalysts, the problems of easy loss of precious metal catalysts and shortage of resources at high temperatures are solved, and high activity and stability are achieved. They are suitable for catalytic combustion of a variety of VOCs, especially benzene and esters. Reduce costs and simplify processes.

CN119075978APending Publication Date: 2024-12-06北京市科学技术研究院资源环境研究所(北京市土地修复工程技术研究中心)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411220632.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing precious metal catalysts are prone to loss at high temperatures, resulting in catalyst deactivation. The lack of precious metal resources and high price limits their application scope and makes it difficult to effectively catalyze the combustion of different types of volatile organic matter (VOCs) gases.

Method used

Using MOF-zirconium-based noble metal catalyst, MOF material was generated by reacting 1,3,5-benzenetrialic acid H3BTC with ZrClO2·8H2O in DMF/formic acid, and mixed with precious metal solution at room temperature, and then dried and calcined to obtain M. -ZrO2 catalyst, used for catalytic oxidation of VOCs.

Benefits of technology

The prepared catalyst has high activity and stability, low activation temperature and relatively low cost. It is suitable for catalytic combustion of different types of VOCs, especially for benzene and esters, and has a simple and easy to expand production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075978A_ABST
    Figure CN119075978A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalysts, in particular to an MOF-zirconium-based noble metal catalyst for catalytic oxidation of VOCs as well as a preparation method and application of the MOF-zirconium-based noble metal catalyst. The MOF-zirconium-based noble metal catalyst is prepared by taking an MOF material as a precursor, the structural formula of the MOF-zirconium-based noble metal catalyst is M-ZrO2, M is noble metal Ru, Pd or Pt, and the mass percentage of the noble metal is 0.01-10%. The precious metal is introduced by using the metal organic framework, compared with a zirconium-based precious metal catalyst prepared by a traditional method, the dispersity of the precious metal is greatly improved, and the catalyst has high VOCs catalytic combustion activity, particularly excellent toluene catalytic oxidation performance and wide application prospects in the field of organic waste gas catalytic oxidation; meanwhile, the method is simple and feasible in preparation process, mild in preparation condition, low in energy consumption and beneficial to industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a MOF-zirconium-based noble metal catalyst for catalytic oxidation of VOCs, and a preparation method and application thereof. Background Art

[0002] Volatile organic compounds (VOCs) refer to organic compounds with a melting point below room temperature and a boiling point between 50 and 260°C. Their main components are hydrocarbons, nitrogen- and sulfur-containing compounds, oxygenated hydrocarbons, halogenated hydrocarbons, alcohols, aldehydes, ketones, esters, and organic acids. They are a type of organic pollutants that are ubiquitous and complex in composition both indoors and outdoors. From the perspective of the types of industrial VOCs produced by various industries, benzene appears most frequently and has the widest industry distribution. Benzene derivatives such as benzene, toluene, and xylene are important organic solvents and chemical raw materials, and are used in a large number of various industrial processes. Due to the great harm of benzene derivatives to human health, they have become an important indicator for the control and monitoring of VOCs gas emissions.

[0003] Compared with non-precious metal catalysts, precious metal catalysts (such as Pt, Pd and Au, etc.) have the advantages of low ignition temperature, complete combustion and few by-products. However, such catalysts are prone to losing precious metals at high temperatures, resulting in catalyst deactivation. In addition, precious metals are expensive and scarce, which also limits the application of precious metal catalysts to a certain extent. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a MOF-zirconium-based precious metal catalyst for catalytic oxidation of VOCs and a preparation method and application thereof, so as to develop a catalyst with high catalytic activity and strong catalytic stability for catalytic combustion of different types of VOCs while reducing the cost of combustion catalysts.

[0005] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:

[0006] In the first aspect, a MOF-zirconium-based precious metal catalyst for catalytic oxidation of VOCs is provided, which is prepared using a MOF material as a precursor and has a structural formula of M-ZrO2, wherein M is a precious metal Ru, Pd or Pt, and the mass percentage of the precious metal is 0.01% to 10%.

[0007] In a second aspect, a method for preparing a MOF-zirconium-based noble metal catalyst for catalytic oxidation of VOCs is provided, which comprises the following steps:

[0008] (1) Dissolve 1,3,5-benzenetricarboxylic acid H3BTC and ZrClO2·8H2O in a flask containing DMF / formic acid, stir until completely dissolved, use reflux condensation method, quickly heat to 100-130°C, and maintain for 12-48 hours; centrifuge to obtain a white precipitate, wash the precipitate with DMF, and then shake for 10-15 minutes, repeat this operation multiple times, vacuum dynamically dry overnight, and grind to obtain white powder Zr-MOF after drying;

[0009] (2) Take a certain amount of M solution and dissolve it in deionized water, add Zr-MOF powder to the solution, stir at room temperature, centrifuge, and dynamically dry at 80-130°C in vacuum overnight. After drying, grind to obtain powder; calcine the powder at 500-800°C for 2-6h to obtain M-ZrO2-N, where M is a precious metal Ru, Pd or Pt, and N is 500-800°C.

[0010] In a third aspect, a MOF-zirconium-based precious metal catalyst for catalytic oxidation of VOCs is provided for use in the catalytic removal of VOCs gas.

[0011] Furthermore, it is used for the catalytic removal of toluene and aliphatic hydrocarbon VOCs gases, and the specific process is: using air as an oxidant for combustion reaction, and the reaction temperature is 100-700°C.

[0012] The beneficial effects of the present invention are:

[0013] (1) The synthetic materials used in the present invention are relatively cheap and have no secondary pollution; the preparation process is simple and easy to expand production;

[0014] (2) The catalyst prepared by the present invention has high activity and stability, and the reaction activation temperature is low;

[0015] (3) The catalyst prepared by the present invention has high catalytic activity not only for benzene, but also for esters, and has a certain universality. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 XRD diagram of the catalyst prepared in Example 1-4;

[0017] Figure 2 Schematic diagram of the toluene catalytic combustion activity of the catalysts prepared in Examples 1-4;

[0018] Figure 3 This is a schematic diagram of the toluene catalytic combustion activity of the catalysts prepared in Example 3, Example 5, and Example 6;

[0019] Figure 4 This is a schematic diagram of the toluene catalytic combustion stability of the catalyst prepared in Example 3;

[0020] Figure 5 Schematic diagram of the catalytic combustion stability of methyl acetate of the catalysts prepared in Examples 1-4. DETAILED DESCRIPTION

[0021] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0022] Example 1

[0023] (1) 1,3,5-benzenetricarboxylic acid H3BTC (2.52 g) and ZrClO2·8H2O (11.64 g) were dissolved in a flask containing DMF / formic acid (300 mL / 300 mL), stirred for 1 h until completely dissolved, and rapidly heated to 130°C using a reflux condensation method and maintained for 48 h. A white precipitate was obtained by centrifugation (8000 r / min, 5 min), which was washed with DMF and then shaken for 10-15 min. This operation was repeated 3 times, and the mixture was dynamically dried at 80°C overnight in a vacuum, and then ground to obtain a white powder Zr-MOF.

[0024] (2) Take 0.1 ml of 54 mg Pd / ml palladium nitrate solution and dissolve it in 150 ml of deionized water, add 2 g of Zr-MOF powder to the solution, stir at room temperature for 1 hour, centrifuge (8000 r / min, 5 min), wash with water for the last time, dynamically dry at 80°C in vacuum overnight, and grind to obtain powder after drying. The powder is calcined at 500°C at 2.5°C / min for 3 hours to obtain Pd-ZrO2-500 catalyst material.

[0025] Example 2

[0026] (1) 1,3,5-benzenetricarboxylic acid H3BTC (2.52 g) and ZrClO2·8H2O (11.64 g) were dissolved in a flask containing DMF / formic acid (300 mL / 300 mL), stirred for 1 h until completely dissolved, and rapidly heated to 130°C using a reflux condensation method and maintained for 48 h. A white precipitate was obtained by centrifugation (8000 r / min, 5 min), which was washed with DMF and then shaken for 10-15 min. This operation was repeated 3 times, and the mixture was dynamically dried at 80°C overnight in a vacuum, and then ground to obtain a white powder Zr-MOF.

[0027] (2) Take 0.1 ml of 54 mg Pd / ml palladium nitrate solution and dissolve it in 150 ml of deionized water, add 2 g of Zr-MOF powder to the solution, stir at room temperature for 1 hour, centrifuge (8000 r / min, 5 min), wash with water for the last time, dynamically dry at 80°C in vacuum overnight, grind to obtain powder after drying. The powder is calcined at 600°C at 2.5°C / min for 3 hours to obtain Pd-ZrO2-600 catalyst material.

[0028] Example 3

[0029] (1) 1,3,5-benzenetricarboxylic acid H3BTC (2.52 g) and ZrClO2·8H2O (11.64 g) were dissolved in a flask containing DMF / formic acid (300 mL / 300 mL), stirred for 1 h until completely dissolved, and rapidly heated to 130°C using a reflux condensation method and maintained for 48 h. A white precipitate was obtained by centrifugation (8000 r / min, 5 min), which was washed with DMF and then shaken for 10-15 min. This operation was repeated 3 times, and the mixture was dynamically dried at 80°C overnight in a vacuum, and then ground to obtain a white powder Zr-MOF.

[0030] (2) Take 0.1 ml of 54 mg Pd / ml palladium nitrate solution and dissolve it in 150 ml of deionized water, add 2 g of Zr-MOF powder to the solution, stir at room temperature for 1 hour, centrifuge (8000 r / min, 5 min), wash with water for the last time, dynamically dry at 80°C in vacuum overnight, grind to obtain powder after drying. The powder is calcined at 700°C at 2.5°C / min for 3 hours to obtain Pd-ZrO2-700 catalyst material.

[0031] Example 4

[0032] (1) 1,3,5-benzenetricarboxylic acid H3BTC (2.52 g) and ZrClO2·8H2O (11.64 g) were dissolved in a flask containing DMF / formic acid (300 mL / 300 mL), stirred for 1 h until completely dissolved, and rapidly heated to 130°C using a reflux condensation method and maintained for 48 h. A white precipitate was obtained by centrifugation (8000 r / min, 5 min), which was washed with DMF and then shaken for 10-15 min. This operation was repeated 3 times, and the mixture was dynamically dried at 80°C overnight in a vacuum, and then ground to obtain a white powder Zr-MOF.

[0033] (2) Take 0.1 ml of 54 mg Pd / ml palladium nitrate solution and dissolve it in 150 ml of deionized water, add 2 g of Zr-MOF powder to the solution, stir at room temperature for 1 hour, centrifuge (8000 r / min, 5 min), wash with water for the last time, dynamically dry at 80°C in vacuum overnight, grind to obtain powder after drying. The powder is calcined at 800°C at 2.5°C / min for 3 hours to obtain Pd-ZrO2-800 catalyst material.

[0034] Example 5

[0035] (1) 1,3,5-benzenetricarboxylic acid H3BTC (2.52 g) and ZrClO2·8H2O (11.64 g) were dissolved in a flask containing DMF / formic acid (300 mL / 300 mL), stirred for 1 h until completely dissolved, and rapidly heated to 130°C using a reflux condensation method and maintained for 48 h. A white precipitate was obtained by centrifugation (8000 r / min, 5 min), which was washed with DMF and then shaken for 10-15 min. This operation was repeated 3 times, and the mixture was dynamically dried at 80°C overnight in a vacuum, and then ground to obtain a white powder Zr-MOF.

[0036] (2) Take 0.048 ml of 113.5 mg Ru / ml ruthenium chloride solution and dissolve it in 150 ml of deionized water. Add 2 g of Zr-MOF powder to the solution, stir at room temperature for 1 hour, centrifuge (8000 r / min, 5 min), wash with water for the last time, dynamically dry at 80°C in vacuum overnight, and grind to obtain powder after drying. The powder is calcined at 700°C at 2.5°C / min for 3 hours to obtain Ru-ZrO2-700 catalyst material.

[0037] Example 6

[0038] (1) 1,3,5-benzenetricarboxylic acid H3BTC (2.52 g) and ZrClO2·8H2O (11.64 g) were dissolved in a flask containing DMF / formic acid (300 mL / 300 mL), stirred for 1 h until completely dissolved, and rapidly heated to 130°C using a reflux condensation method and maintained for 48 h. A white precipitate was obtained by centrifugation (8000 r / min, 5 min), which was washed with DMF and then shaken for 10-15 min. This operation was repeated 3 times, and the mixture was dynamically dried at 80°C overnight in a vacuum, and then ground to obtain a white powder Zr-MOF.

[0039] (2) Take 0.068 ml of 80.7 mg Pt / ml chloroplatinic acid solution and dissolve it in 150 ml of deionized water. Add 2 g of Zr-MOF powder to the solution, stir at room temperature for 1 hour, centrifuge (8000 r / min, 5 min), wash with water for the last time, dynamically dry at 80°C in vacuum overnight, and grind to obtain powder after drying. The powder is calcined at 700°C at 2.5°C / min for 3 hours to obtain Pt-ZrO2-700 catalyst material.

[0040] Example 1-4 After the zirconium-based metal organic framework material is impregnated into the noble metal solution, it is taken out, dried, and calcined at 500°C, 600°C, 700°C or 800°C for 3 hours to obtain zirconium-based noble metal catalysts: M-ZrO2-500, M-ZrO2-600, M-ZrO2-700 and M-ZrO2-800. Figure 1 As shown, the prepared catalyst is a mixed phase of monoclinic and tetragonal zirconium dioxide crystal phases. With the increase of calcination temperature, the monoclinic phase increases and the tetragonal phase decreases.

[0041] Figure 2-3 The specific test conditions are as follows: toluene concentration is 1000ppm, the rest is air, and the total flow rate is 300mL min -1 , the reaction mass space velocity is 180,000 mL·h -1 ·g -1 The specific process is: using air as an oxidant to carry out combustion reaction, catalytic combustion of toluene, the reaction temperature is 100 ~ 700 ℃. The stability results are as follows Figure 4 shown.

[0042] Figure 5 The catalytic activity of methyl acetate was determined under the following conditions: the concentration of methyl acetate was 400 ppm, the rest was air, and the total flow rate was 300 mL min -1 , the reaction mass space velocity is 180,000 mL·h -1 ·g -1 The specific process is: using air as an oxidant to carry out a combustion reaction to catalyze the combustion of methyl acetate, and the reaction temperature is 100 to 700°C.

[0043] The present invention utilizes a metal organic framework to introduce precious metals, which greatly improves the dispersion of precious metals compared to zirconium-based precious metal catalysts prepared by traditional methods. The catalyst has high VOCs catalytic combustion activity, especially excellent catalytic oxidation of toluene, and has broad application prospects in the field of catalytic oxidation of organic waste gas. At the same time, the method of the present invention has a simple and easy preparation process, mild preparation conditions, low energy consumption, and is conducive to industrial large-scale production.

[0044] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0045] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A MOF-zirconium-based noble metal catalyst for catalytic oxidation of VOCs, characterized in that: It is prepared with MOF material as a precursor, and has a structural formula of M-ZrO2, wherein M is a noble metal such as Ru, Pd or Pt, and the mass percentage of the noble metal is 0.01% to 10%.

2. A method for preparing a MOF-zirconium-based noble metal catalyst for catalytic oxidation of VOCs, characterized in that: The following steps are involved: (1) Dissolve 1,3,5-benzenetricarboxylic acid H3BTC and ZrClO2·8H2O in a flask containing DMF / formic acid, stir until completely dissolved, use reflux condensation method, quickly heat to 100-130°C, and maintain for 12-48 hours; centrifuge to obtain a white precipitate, wash the precipitate with DMF, and then shake for 10-15 minutes, repeat this operation multiple times, vacuum dynamically dry overnight, and grind to obtain white powder Zr-MOF after drying; (2) Take a certain amount of M solution and dissolve it in deionized water, add Zr-MOF powder to the solution, stir at room temperature, centrifuge, and dynamically dry at 80-130°C in vacuum overnight. After drying, grind to obtain powder; calcine the powder at 500-800°C for 2-6h to obtain M-ZrO2-N, where M is a precious metal Ru, Pd or Pt, and N is 500-800°C.

3. Use of the MOF-zirconium-based noble metal catalyst for catalytic oxidation of VOCs according to claim 1 in the catalytic removal of VOCs gas.

4. The use according to claim 3, characterized in that: Used for catalytic removal of toluene and aliphatic hydrocarbon VOCs gases, the specific process is: using air as an oxidant for combustion reaction, the reaction temperature is 100 ~ 700 ℃.