Catalyst for preparing lactic acid by dehydrogenation of ethylene glycol as well as preparation method and application of catalyst

By using the catalyst M/S@C in ethylene glycol dehydrogenation to lactic acid, the problems of low catalyst utilization rate and equipment corrosion in the stirred tank are solved, and efficient lactic acid is achieved, which is suitable for fixed bed reactions. simplifies the process and improves production efficiency.

CN119075981AActive Publication Date: 2024-12-06CHINA ENERGY INVESTMENT CORP LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310634226.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-06
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

During the process of polyol lactic acid production, the presence of "dead corners" in the stirred tank leads to low catalyst utilization, serious corrosion of liquid alkali on the equipment, and complex solid-liquid separation, and lacks suitable catalysts for fixed bed reactors.

Method used

Using catalyst M/S@C, M is the active component (such as Ru, Sn) and S@C is the solid alkali support. By coating the alkali oxide shell, a catalyst suitable for fixed bed reactors is prepared to avoid Use liquid alkali to improve catalytic performance.

Benefits of technology

It improves the activity and utilization of the catalyst, avoids equipment corrosion, simplifies discharge treatment, simple process and high production efficiency, and achieves efficient ethylene glycol dehydrogenation to produce lactic acid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004259365880000071
    Figure BDA0004259365880000071
  • Figure BDA0004259365880000091
    Figure BDA0004259365880000091
Patent Text Reader

Abstract

The invention provides a catalyst for preparing lactic acid through ethylene glycol dehydrogenation. The general formula of the catalyst is M / S-C, wherein M is an active component and is selected from any one or a combination of more of Ru, Ir, Sn, Rh, Pd, Ag, Cd, In and Sb; s (at) C is a solid alkali carrier, and C is a carrier and is selected from any one or a combination of more of Al2O3, SiO2 and ZrO2; s is a basic oxide shell layer coated on the surface of C and is selected from any one or a combination of more of BeO, MgO, CaO, SrO, BaO and RaO; on the basis of the mass of C, the mass of M is 0.75-30 wt%, and the mass of S is 2-15 wt%. The invention also provides a preparation method of the catalyst, and application and a method of the catalyst in preparation of lactic acid through ethylene glycol dehydrogenation. The catalyst can be used for preparing lactic acid through ethylene glycol dehydrogenation, is high in activity and is suitable for being used in a fixed bed reactor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparing lactic acid by dehydrogenating alcohol, and particularly relates to a catalyst used in preparing lactic acid by dehydrogenating ethylene glycol, and a preparation method and application thereof. Background Art

[0002] At present, the production of lactic acid from polyols is carried out in stirred tanks, but there are three disadvantages in stirred tanks: (1) no matter how the stirring is done, there is always a "dead corner" at the bottom of the reactor, and solid particles will inevitably precipitate, resulting in low catalyst utilization; (2) liquid alkali is used during the process, and liquid alkali seriously corrodes the equipment; (3) it is difficult to separate the solid-liquid mixture discharged from the reactor. When other reaction devices are used, there is no suitable catalyst. Summary of the invention

[0003] The first object of the present invention is to provide a catalyst for preparing lactic acid by dehydrogenating ethylene glycol, which catalyst can be used in preparing lactic acid by dehydrogenating ethylene glycol, has high activity, and is suitable for use in a fixed bed reactor;

[0004] The second object of the present invention is to provide a method for preparing the above-mentioned catalyst;

[0005] The third object of the present invention is to provide an application of the above catalyst in the dehydrogenation of ethylene glycol to produce lactic acid;

[0006] The fourth object of the present invention is to provide a method for preparing lactic acid by dehydrogenating ethylene glycol.

[0007] To achieve the first object of the present invention, the following technical solutions are adopted:

[0008] A catalyst for preparing lactic acid by dehydrogenating ethylene glycol, the general formula of which is M / S@C; wherein:

[0009] M is an active component, selected from any one or more combinations of Ru, Ir, Sn, Rh, Pd, Ag, Cd, In and Sb;

[0010] S@C is a solid alkali carrier, C is a carrier, and is selected from any one or more combinations of Al2O3, SiO2 and ZrO2; S is an alkaline oxide shell layer coated on the surface of C, and is selected from any one or more combinations of BeO, MgO, CaO, SrO, BaO and RaO;

[0011] Based on the mass of C, the mass of M is 0.75-30wt%, such as 1wt%, 1.5wt%, 2wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt% and 28wt%, and any value within this range; the mass of S is 2-15wt%, such as 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt% and 14wt%, and any value within this range.

[0012] The catalyst of the invention can be used in the preparation of lactic acid by dehydrogenation of ethylene glycol, and is suitable for use in a fixed bed reactor due to its high activity.

[0013] To improve the catalytic performance of the catalyst, in one embodiment, M includes Ru and Sn.

[0014] In one embodiment, the mass of Ru in M ​​is 0.5-10wt%, such as 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt% and 9wt%, and any value within the range, based on the mass of C.

[0015] In one embodiment, in M, the mass ratio of Ru to Sn is 1:(0.4-3), such as 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, 1:2.2, 1:2.4, 1:2.6 and 1:2.8, and any ratio within this range.

[0016] In order to improve the catalytic performance of the catalyst, in one embodiment, C is a granular carrier with a double pore distribution.

[0017] In one embodiment, the pore sizes of the double pores are 5-50nm (e.g., 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm and 45nm) and 100-300nm (e.g., 120nm, 140nm, 160nm, 180nm, 200nm, 220nm, 240nm, 260nm and 280nm).

[0018] In one embodiment, the average pore sizes of the double pores are 20±4 nm and 200±10 nm, respectively.

[0019] The catalyst of the invention has high activity and good catalytic performance, can be used in preparing lactic acid by dehydrogenating ethylene glycol, and is suitable for use in a fixed bed reactor.

[0020] In order to achieve the second object of the present invention, a method for preparing the above-mentioned catalyst is provided.

[0021] In one embodiment, the steps include:

[0022] (1) dissolving the salt corresponding to the oxide shell S in deionized water to obtain a shell impregnation solution;

[0023] (2) impregnating the carrier C in the shell impregnation solution obtained in step (1), and then filtering, drying and calcining in sequence to obtain a solid alkali carrier S@C;

[0024] (3) dissolving the salt corresponding to the active component M in deionized water to obtain an active component impregnation solution;

[0025] (4) The solid base carrier S@C obtained in step (2) is immersed in the active component impregnation solution obtained in step (3), and then a formaldehyde aqueous solution is added thereto to cause a reduction reaction, and then the solid base carrier S@C is filtered, washed and dried in sequence to obtain a catalyst M / S@C.

[0026] Those skilled in the art will appreciate that the filtration in step (2) and step (4) may be carried out by any filtration method commonly used in the art, such as suction filtration, plate and frame filtration, sedimentation separation, etc. In one embodiment, suction filtration is used.

[0027] In order to improve the catalytic performance of the prepared catalyst, in one embodiment, in step (1), the salt corresponding to the oxide shell S is selected from any one or a combination of nitrates, chlorides and sulfates of Be, Mg, Ca, Sr, Ba and Ra, such as Ba(NO3)2, BaCl2, CaCl2, MgSO4, Sr(NO3)2, etc.

[0028] Those skilled in the art will appreciate that in step (1), the salt may be a salt containing crystalline water or a salt not containing crystalline water.

[0029] To improve the catalytic performance of the prepared catalyst, in one embodiment, in step (1), the concentration of the shell impregnation solution is 0.05-0.5 mmol / ml, such as 0.07 mmol / ml, 0.1 mmol / ml, 0.15 mmol / ml, 0.2 mmol / ml, 0.25 mmol / ml, 0.3 mmol / ml, 0.35 mmol / ml, 0.4 mmol / ml and 0.45 mmol / ml, and any value within this range.

[0030] To improve the impregnation effect of the shell layer, in one embodiment, in step (2), the impregnation temperature is 20-50°C, such as 25°C, 30°C, 35°C, 40°C and 45°C, and any temperature within this range; the impregnation time is 24-72h, such as 30h, 36h, 42h, 48h, 54h, 60h and 66h, and any value within this range.

[0031] To improve the coating effect of the shell layer, in one embodiment, in step (2), the drying temperature is 60-100°C, such as 65°C, 70°C, 75°C, 80°C, 85°C, 90°C and 95°C, and any temperature within this range; the drying time is 12-36h, such as 14h, 16h, 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h and 34h, and any value within this range.

[0032] To improve the coating effect of the shell layer, in one embodiment, in step (2), the calcination temperature is 400-600°C, such as 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C and 580°C, and any temperature within this range; the calcination time is 2-6h, such as 2.5h, 3h, 3.5h, 4h, 4.5h, 5h and 5.5h, and any value within this range.

[0033] To improve the impregnation effect of the active component, in one embodiment, in step (3), the concentration of the active component impregnation solution is 0.05-0.5mmol / ml, such as 0.07mmol / ml, 0.1mmol / ml, 0.15mmol / ml, 0.2mmol / ml, 0.25mmol / ml, 0.3mmol / ml, 0.35mmol / ml, 0.4mmol / ml and 0.45mmol / ml, as well as any value within this range.

[0034] In one embodiment, in step (3), the salt corresponding to the active component M is selected from any one or more combinations of nitrates, chlorides and sulfates of Ru, Sn, Rh, Ir, Pd, Ag, Cd, In and Sb, such as RuCl3·3H2O, H2IrCl6·6H2O, SnCl2·2H2O, In(NO3)2, PdSO4 and SbCl2.

[0035] Those skilled in the art will appreciate that in step (3), the salt may be a salt containing water of crystallization or a salt not containing water of crystallization.

[0036] To improve the impregnation effect of the active components, in one embodiment, in step (4), the impregnation temperature is 20-50°C, such as 25°C, 30°C, 35°C, 40°C and 45°C, and any temperature within this range; the impregnation time is 6-18h, such as 8h, 10h, 12h, 14h and 16h, and any value within this range.

[0037] In order to reduce the salt corresponding to the active component M to the active component M, in one embodiment, in step (4), the reduction temperature is 40-60°C, such as 45°C, 50°C and 55°C, and any temperature within the range; the reduction time is 0.5-1.5h, such as 1h, and any value within the range.

[0038] In order to improve the reduction effect, in one embodiment, in step (4), the concentration of the formaldehyde aqueous solution is 5-15wt%, such as 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt% and 14wt%, and any value within this range.

[0039] To improve the loading effect of the active components, in one embodiment, in step (4), the drying temperature is 60-100°C, such as 65°C, 70°C, 75°C, 80°C, 85°C, 90°C and 95°C, and any temperature within this range; the drying time is 2-5h, such as 2.5h, 3h, 3.5h, 4h and 4.5h, and any value within this range.

[0040] In order to improve the catalytic performance of the prepared catalyst, in one embodiment, the amounts of the active component M, the salt corresponding to the oxide shell S and the carrier C satisfy the following conditions: based on the mass of C, the mass of M is 0.75-30wt%, such as 1wt%, 1.5wt%, 2wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt% and 28wt%, and any value within the range; the mass of S is 2-15wt%, such as 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt% and 14wt%, and any value within the range.

[0041] To achieve the third object of the present invention, the present invention provides the above catalyst and the use of the catalyst prepared according to the above preparation method in the dehydrogenation of ethylene glycol to produce lactic acid.

[0042] To achieve the fourth object of the present invention, a method for preparing lactic acid by dehydrogenating ethylene glycol is provided, comprising:

[0043] Ethylene glycol and methanol are mixed and passed through a fixed bed reactor from bottom to top, and a catalytic dehydrogenation reaction is carried out on the catalyst bed therein to produce lactic acid; wherein,

[0044] The catalyst used is the aforementioned catalyst or a catalyst prepared according to the aforementioned preparation method.

[0045] Those skilled in the art understand that when a fixed bed reactor is used to carry out the reaction of dehydrogenating ethylene glycol to produce lactic acid, the raw materials are fed from the lower part of the fixed bed reactor and the products are discharged from the upper part of the fixed bed reactor.

[0046] The present invention adopts the above-mentioned catalyst and a fixed bed reactor to carry out the reaction of preparing lactic acid from ethylene glycol by dehydrogenation, thereby realizing the preparation of lactic acid from ethylene glycol by dehydrogenation. On the one hand, the fixed bed reactor is used to carry out the reaction of preparing lactic acid from ethylene glycol by dehydrogenation, so that the "dead corner" problem existing when a stirred kettle is used to carry out the reaction can be avoided, and the utilization rate of the catalyst is improved. Moreover, the discharge does not require solid-liquid separation, the process is simple, and the production efficiency is high. On the other hand, in the process of preparing lactic acid from ethylene glycol by dehydrogenation, the above-mentioned catalyst of the present invention is used to catalyze the dehydrogenation of ethylene glycol, the catalyst has high activity and can be applied to the fixed bed reactor, and the catalyst carrier is a solid alkali carrier, so the use of liquid alkali is avoided, thereby avoiding the corrosion of the equipment by alkali solution.

[0047] In one embodiment, the molar ratio of methanol to ethylene glycol is (1-4):1, such as 1.5:12:1, 2.5:1, 3:1 and 3.5:1, and any ratio within this range.

[0048] In one embodiment, the feed volume space velocity of ethylene glycol is 0.1-2h -1 , for example 0.2h -1 、0.4h -1 、0.6h -1 , 0.8h -1 , 1h -1 , 1.2h -1 , 1.4h -1 , 1.6h -1 and 1.8h -1 , and any value in this range.

[0049] In one embodiment, the reaction temperature is 100-200°C, such as 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C and 190°C, and any temperature within this range; the reaction pressure is 0.1-3MPa, such as 0.2MPa, 0.4MPa, 0.6MPa, 0.8MPa, 1MPa, 1.2MPa, 1.4MPa, 1.6MPa, 1.8MPa, 2MPa, 2.2MPa, 2.4MPa, 2.6MPa and 2.8MPa, and any value within this range.

[0050] The beneficial effects of the present invention are:

[0051] The catalyst used in the process of preparing lactic acid by dehydrogenating ethylene glycol has high activity, good catalytic performance, and alkalinity, and can be used in the process of preparing lactic acid by dehydrogenating ethylene glycol. The catalyst is suitable for use in a fixed bed reactor, and does not require the addition of liquid alkali, thereby preventing the corrosion of the equipment by the liquid alkali.

[0052] The method for preparing the above-mentioned catalyst of the present invention is simple and can easily obtain a catalyst with high activity and good catalytic performance;

[0053] The catalyst of the present invention can be applied to the process of preparing lactic acid from ethylene glycol by dehydrogenation, and the method of preparing lactic acid from ethylene glycol by dehydrogenation is to use the catalyst and a fixed bed reactor to carry out the reaction of preparing lactic acid from ethylene glycol by dehydrogenation, thereby realizing the process of preparing lactic acid from ethylene glycol by dehydrogenation. On the one hand, the fixed bed reactor is used to carry out the reaction of preparing lactic acid from ethylene glycol by dehydrogenation, thereby avoiding the problem of "dead corner" existing when a stirred tank is used to carry out the reaction, thereby improving the utilization rate of the catalyst, and the discharge does not require solid-liquid separation, thus the process is simple and the production efficiency is high. On the other hand, in the process of preparing lactic acid from ethylene glycol by dehydrogenation, the catalyst of the present invention is used to carry out catalytic dehydrogenation of ethylene glycol, the catalyst has high activity and can be applied to a fixed bed reactor, and the catalyst carrier is a solid alkali carrier, thereby avoiding the use of liquid alkali, thereby avoiding the corrosion of the equipment by alkali solution. DETAILED DESCRIPTION

[0054] The technical scheme and its effects of the present invention are further described below in conjunction with specific implementation methods / examples. The following implementation methods / examples are only used to illustrate the content of the present invention, and the invention is not limited to the following implementation methods or examples. Simple changes made to the present invention using the concept of the present invention are all within the scope of protection claimed by the present invention.

[0055] The main raw materials used in the following examples and comparative examples are shown in Table 1:

[0056] Table 1 Main raw materials used in the examples of the present invention and comparative examples

[0057]

[0058] The catalyst performance test method is as follows:

[0059] 1. The content of active components in the catalyst is tested by X-ray fluorescence spectrometer (XRF);

[0060] 2. Ethylene glycol conversion and lactic acid selectivity:

[0061] Assume that the original molar amount of ethylene glycol in the system before the reaction is n1, the molar amount of ethylene glycol in the system after the reaction is n2, and the molar amount of lactic acid in the system after the reaction is n3, then

[0062] The molar amount of ethylene glycol converted = n1-n2;

[0063] Ethylene glycol conversion rate = (n1-n2) / n1×100%;

[0064] Lactic acid selectivity = n3 / (n1-n2)×100%.

[0065] Example 1 (S1)

[0066] Catalyst A1 for use in dehydrogenation of ethylene glycol to produce lactic acid was prepared according to the following preparation method:

[0067] (1) Dissolve 2.6 g of Ba(NO3)2 (the salt corresponding to the oxide shell S) in 50 ml of deionized water to obtain a shell impregnation solution with a concentration of 0.199 mmol / ml;

[0068] (2) placing the bi-porous distributed granular alumina carrier K1 (carrier C) in the shell impregnation solution obtained in step (1) at room temperature (25° C.) for 48 hours, and then successively performing suction filtration (filtration), drying at 85° C. for 24 hours, and calcining at 500° C. for 4 hours to obtain a solid alkali carrier S@C;

[0069] (3) Dissolve 2.05 g of RuCl3·3H2O and 1.9 g of SnCl2·2H2O (the salt corresponding to the active component M) in 50 ml of deionized water to obtain a Ru solution with a concentration of 0.155 mmol / ml. 3+ and 0.168mmol / ml Sn 2+ Active ingredient impregnation solution;

[0070] (4) 25 g of the solid alkali carrier S@C obtained in step (2) was placed in the active component impregnation solution obtained in step (3) and immersed at room temperature (25° C.) for 12 h, and then 100 ml of a 10 wt% formaldehyde aqueous solution was added thereto and reduced at 50° C. for 1 h to reduce Ru 3+ and Sn 2+Reduced to elemental Ru and Sn, then filtered, washed with deionized water, and dried at 90 °C for 3 h to obtain the catalyst Ru(3.4)-Sn(4.2) / BaO(6.5)@Al2O3 (catalyst M / S@C), denoted as catalyst A1;

[0071] The obtained catalyst A1, namely Ru(3.4)-Sn(4.2) / BaO(6.5)@Al2O3, is based on the mass of the carrier C.

[0072] In the active component M, the content of Ru is 3.4wt% and the content of Sn is 4.2wt%;

[0073] In the oxide shell layer S, the content of BaO is 6.5 wt%.

[0074] Catalyst A2-7 was prepared according to the preparation method of Example 1; the reaction raw materials and reaction conditions of each step are shown in Table 2. Among them,

[0075] Catalyst A2 is Ru(0.8)-Sn(1.1) / BaO(2)@Al2O3;

[0076] Catalyst A3 is Ru(2)-Sn(2.5) / BaO(3)@Al2O3;

[0077] Catalyst A4 is Ru(0.5)-Sn(1) / BaO(2)@Al2O3;

[0078] Catalyst A5 is Ru(10)-Sn(5) / BaO(15)@Al2O3;

[0079] Catalyst A6 is In(10)-Sb(20) / MgO(10)@ZrO2;

[0080] Catalyst A7 is Sb(18) / SrO(8)@SiO2;

[0081] Table 2 Reaction materials and reaction conditions of each step of Example 1-7 (S1-7)

[0082]

[0083] Application Example 1-7 (Y1-7)

[0084] The catalyst A1-7 obtained in Example 1-7 was applied to the dehydrogenation of ethylene glycol to produce lactic acid, as follows:

[0085] Ethylene glycol and methanol are mixed and passed through a fixed bed reactor from bottom to top, and a catalytic dehydrogenation reaction is carried out on the catalyst bed therein to produce lactic acid. The reaction conditions and reaction results are shown in Table 3.

[0086] Table 3 Reaction conditions and reaction results of application examples 1-7 (Y1-7)

[0087] Application Examples Y1 Y2 Y3 Y4 Y5 Y6 Y7 catalyst A1 A2 A3 A4 A5 A6 A7 Molar ratio of methanol to ethylene glycol 2:1 1:1 4:1 3:1 1.5:1 2:1 2:1 <![CDATA[The feed volume space velocity of ethylene glycol (h -1 )]]> 1 0.1 2 1.5 0.5 1 1 Reaction temperature (℃) 150 100 200 120 180 150 150 Reaction pressure (MPa) 1.5 0.1 3 1 2 1.5 1.5 Ethylene glycol conversion rate (%) 99 96 97 96 97 95 94 Lactic acid selectivity (%) 99 96 98 96 97 94 94

[0088] According to Application Examples 1-7 and Table 3, when the catalyst A1-7 prepared in Examples 1-7 of the present invention is used to carry out the reaction of ethylene glycol dehydrogenation to produce lactic acid in a fixed bed reactor, the catalyst activity is high, the conversion rate of ethylene glycol reaches 94-99%, the selectivity of lactic acid reaches 94-99%, and the related problems existing when using a stirred tank are avoided.

Claims

1. A catalyst for preparing lactic acid by dehydrogenating ethylene glycol, characterized in that: The general formula of the catalyst is M / S@C; wherein, M is an active component, selected from any one or more combinations of Ru, Ir, Sn, Rh, Pd, Ag, Cd, In and Sb; S@C is a solid alkali carrier, C is a carrier, and is selected from any one or more combinations of Al2O3, SiO2 and ZrO2; S is an alkaline oxide shell layer coated on the surface of C, and is selected from any one or more combinations of BeO, MgO, CaO, SrO, BaO and RaO; Based on the mass of C, the mass of M is 0.75-30 wt%, and the mass of S is 2-15 wt%.

2. The catalyst according to claim 1, characterized in that M includes Ru and Sn.

3. The catalyst according to claim 2, characterized in that The mass of Ru in M ​​is 0.5-10 wt% based on the mass of C; and / or In M, the mass ratio of Ru to Sn is 1:(0.4-3).

4. The catalyst according to claim 2 or 3, characterized in that C is a granular carrier with double pore distribution.

5. The catalyst according to claim 4, characterized in that The pore sizes of the double pores are 5-50 nm and 100-300 nm respectively; and / or The average pore diameters of the double pores are 20±4 nm and 200±10 nm respectively.

6. A method for preparing the catalyst according to any one of claims 1 to 5.

7. The preparation method according to claim 6, characterized in that: The following steps are involved: (1) dissolving the salt corresponding to the oxide shell S in deionized water to obtain a shell impregnation solution; (2) impregnating the carrier C in the shell impregnation solution obtained in step (1), and then filtering, drying and calcining in sequence to obtain a solid alkali carrier S@C; (3) dissolving the salt corresponding to the active component M in deionized water to obtain an active component impregnation solution; (4) placing the solid base carrier S@C obtained in step (2) in the active component impregnation solution obtained in step (3) for immersion, then adding formaldehyde aqueous solution thereto to cause a reduction reaction, and then filtering, washing and drying in sequence to obtain a catalyst M / S@C; Preferably, in step (1), the salt corresponding to the oxide shell S is selected from any one or a combination of nitrates, chlorides and sulfates of Be, Mg, Ca, Sr, Ba and Ra; and / or In step (2), the calcination temperature is 400-600° C. and the calcination time is 2-6 hours; and / or In step (4), the reduction temperature is 40-60° C. and the reduction time is 0.5-1.5 h; and / or In step (4), the concentration of the formaldehyde aqueous solution is 5-15 wt %.

8. Use of the catalyst according to any one of claims 1 to 5 and the catalyst prepared according to the preparation method according to claim 7 or 8 in the dehydrogenation of ethylene glycol to produce lactic acid.

9. A method for preparing lactic acid by dehydrogenating ethylene glycol, characterized in that: The method comprises: Ethylene glycol and methanol are mixed and passed through a fixed bed reactor from bottom to top, and a catalytic dehydrogenation reaction is carried out on the catalyst bed therein to produce lactic acid; wherein, The catalyst used is the catalyst described in any one of claims 1 to 5 or the catalyst prepared according to the preparation method described in claim 7 or 8.

10. The method according to claim 9, characterized in that The molar ratio of methanol to ethylene glycol is (1-4):1; and / or The reaction temperature is 100-200°C and the reaction pressure is 0.1-3MPa.

Citation Information

Patent Citations

  • Macropore-mesopore ordered magnesium-aluminum composite oxide material and preparation method thereof

    CN106995215A

  • Method for preparing acid by catalyzing and dehydrogenizing alcohol under solvent-free condition

    CN109627155A

  • Method for preparing lactic acid through selective catalytic conversion of ethylene glycol

    CN110357770A

  • Copper-supported catalyst and method of producing the same, method of producing lactic acid, and method of producing formic acid

    JP2015134324A