Preparation method of nanosheet hydrotalcite catalyst and application of nanosheet hydrotalcite catalyst in absorption of carbon dioxide by alcohol amine solution

By calcining the ultrasonic hydrothermal reaction of urea, nickel and aluminum salts at high temperatures, an efficient nanosheet hydrotalcite catalyst was prepared, which solved the problems of high structural stability and energy consumption of hydrotalcite catalysts in high temperature environments, and achieved alcohol The effect of efficient carbon dioxide absorption in amine solution.

CN119075989APending Publication Date: 2024-12-06CHN ENERGY NEW ENERGY TECHNOLOGY RESEARCH INSTITUTE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411180843.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing hydrotalcite catalysts may undergo structural damage or decrease in activity when used in high temperature, high pressure or corrosive environments, limiting their stability in industrial-scale applications and high energy consumption during carbon dioxide absorption.

Method used

Under ultrasonic conditions, urea, nickel salt and aluminum salt are mixed with organic solvents, hydrothermal reaction and calcination are carried out to prepare a nanosheet hydrotalcite catalyst. This catalyst has a high specific surface area, multi-active sites and structural stability, and is used for Carbon dioxide is absorbed in alcohol amine solution.

Benefits of technology

The reaction rate and absorption efficiency of alcohol amines and carbon dioxide are improved, energy consumption is reduced, and the stability and selectivity of the catalyst are improved, which significantly improves the carbon dioxide capture efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of carbon capture, and discloses a preparation method of a nanosheet hydrotalcite catalyst and application of the nanosheet hydrotalcite catalyst in absorption of carbon dioxide by an alcohol amine solution. The method comprises the following steps that (1) urea, nickel salt, aluminum salt and a mixed solvent are mixed under the ultrasonic condition, a mixed solution is obtained, the mixed solvent contains an organic solvent and water, and the organic solvent is selected from at least one of ethanolamine, N-methyldiethanolamine, n-hexadecanol and n-hexanol; and (2) carrying out hydrothermal reaction on the mixed solution, and calcining the obtained reaction product. The nanosheet hydrotalcite catalyst prepared by the method is high in structural stability and high in activity, and the absorption efficiency and selectivity can be improved in the process of catalyzing an alcohol amine solution to absorb carbon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon capture, and in particular to a method for preparing a nano-sheet hydrotalcite catalyst and application of the catalyst in absorbing carbon dioxide with an alcohol amine solution. Background Art

[0002] In recent years, with the increasing severity of global climate change, reducing carbon dioxide emissions has become the focus of attention of all countries. Carbon dioxide capture, utilization and storage (CCUS) technology is considered an important means to achieve a low-carbon economy. Carbon dioxide capture methods mainly include physical absorption, chemical absorption and membrane separation. Among them, chemical absorption has become a hot topic in current research due to its high selectivity and absorption efficiency. The chemical absorption method mainly separates carbon dioxide from the gas mixture through a chemical reaction between the absorbent and carbon dioxide. In this process, amine solution, as a commonly used absorbent, has broad application prospects.

[0003] The efficiency of amine solution in absorbing carbon dioxide is limited by its chemical reaction rate. In order to improve the absorption efficiency, researchers are committed to developing efficient catalysts. At present, catalyst research and development mainly focuses on the following aspects: (1) improving the molecular structure of amine and improving its reaction activity with carbon dioxide; (2) developing new multifunctional catalysts to achieve efficient absorption of carbon dioxide; (3) studying the stability, anti-toxicity and regeneration performance of catalysts. In recent years, researchers have made some progress in catalyst research and development, but there are still certain challenges.

[0004] As a new type of catalyst, hydrotalcite compounds show good application prospects in the field of carbon dioxide absorption. Hydrotalcite compounds have a unique layered structure, abundant surface active sites and high catalytic activity. Applying them to the process of carbon dioxide absorption by alcohol amine solution can effectively improve the absorption efficiency. At present, researchers have successfully applied hydrotalcite compounds to carbon dioxide absorption and have achieved certain research results.

[0005] Although the technology of absorbing carbon dioxide with alcohol amine solution has made certain progress in research and application, the following problems still exist: (1) The selectivity and stability of the absorbent need to be improved; (2) The activity, anti-toxicity and regeneration performance of the catalyst need to be optimized; (3) The carbon dioxide absorption process has high energy consumption and high cost. To address the above problems, the following solutions can be taken: (1) Screen and optimize the absorbent to improve its selectivity and stability; (2) Further study the structure-activity relationship of the catalyst and develop an efficient and stable catalyst; (3) Optimize the carbon dioxide absorption process to reduce energy consumption and cost.

[0006] In short, carbon dioxide capture technology is of great significance. By continuously optimizing the research and development of catalysts for the absorption of carbon dioxide by alcohol amine solutions and improving the application of hydrotalcite compounds in catalytic carbon dioxide absorption, it is expected to provide strong support for achieving carbon emission reduction goals.

[0007] Although some progress has been made in the research on hydrotalcite-promoted carbon dioxide absorption by alcohol amines, there are still some problems and challenges, mainly including the following aspects: hydrotalcite catalysts may suffer structural damage or reduced activity during recycling, especially under high temperature, high pressure or corrosive environment. This limits its stability in industrial-scale applications. The absorption and desorption process of carbon dioxide usually requires high energy consumption. How to reduce energy consumption while ensuring absorption efficiency is an important issue facing the technology of hydrotalcite-promoted carbon dioxide absorption by alcohol amines. Summary of the invention

[0008] The purpose of the present invention is to overcome the problem that the existing hydrotalcite may be structurally damaged or its activity may be reduced during use under high temperature, high pressure or corrosive environment, which limits its stability in industrial-scale application, and provide a method for preparing a nano-sheet hydrotalcite catalyst and its application in the absorption of carbon dioxide by an alcohol amine solution. The nano-sheet hydrotalcite catalyst prepared by the method has high structural stability and high activity, and has good absorption efficiency and selectivity in the process of catalyzing the absorption of carbon dioxide by an alcohol amine solution.

[0009] In order to achieve the above object, the present invention provides a method for preparing a nanosheet hydrotalcite catalyst, which comprises the following steps: (1) mixing urea, nickel salt, aluminum salt and a mixed solvent under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains an organic solvent and water, and the organic solvent is selected from at least one of ethanolamine, N-methyldiethanolamine, n-hexadecanol and n-hexanol; (2) subjecting the mixed solution to a hydrothermal reaction, and then calcining the obtained reaction product.

[0010] Preferably, in the mixed solvent, the volume ratio of the water to the organic solvent is 2-6:1.

[0011] Preferably, in step (1), the ultrasonic conditions include: the ultrasonic frequency is 80-120 kHz, the ultrasonic power is 500-700 W, and the ultrasonic time is 5-15 min.

[0012] Preferably, in step (1), the amount of urea used is 0.1-2 mol based on 1000 mL of the mixed solvent.

[0013] Preferably, in step (1), the nickel salt is calculated as Ni, the aluminum salt is calculated as Al, and the molar ratio of the urea, the nickel salt and the aluminum salt is 5-30:2-4:1.

[0014] Preferably, the nickel salt is selected from at least one of nickel nitrate, nickel chloride and nickel sulfate.

[0015] Preferably, the aluminum salt is selected from at least one of aluminum nitrate, aluminum chloride and aluminum sulfate.

[0016] Preferably, in step (2), the conditions of the hydrothermal reaction include: temperature of 130-200° C. and time of 4-8 h.

[0017] Preferably, in step (2), the calcination conditions include: temperature of 400-600° C. and time of 2-5 h.

[0018] The second aspect of the present invention provides a nanosheet hydrotalcite catalyst prepared by the method described above.

[0019] Preferably, the specific surface area of ​​the hydrotalcite catalyst is 216-258 m 2 / g.

[0020] The third aspect of the present invention provides a use of a nanosheet hydrotalcite catalyst prepared by the method described above or the nanosheet hydrotalcite catalyst described above in absorbing carbon dioxide with an alcoholamine solution.

[0021] A fourth aspect of the present invention provides a method for absorbing carbon dioxide, the method comprising the following steps: S1, mixing the alcohol amine solution with the catalyst to obtain a carbon dioxide absorption liquid; S2, contacting the carbon dioxide absorbing liquid with the carbon dioxide mixed gas at 30-50° C. and normal pressure to absorb carbon dioxide in the carbon dioxide mixed gas; S3, after the absorption is completed, the carbon dioxide absorption liquid is desorbed at 90-115° C. and normal pressure; Wherein, the catalyst is the nanosheet hydrotalcite catalyst prepared by the method described above or the nanosheet hydrotalcite catalyst described above.

[0022] Preferably, in step S1, the alcoholamine compound in the alcoholamine solution is selected from at least two of ethanolamine, N-methyldiethanolamine and 2-amino-2-methyl-1-propanol.

[0023] Preferably, in step S1, the concentration of the alcoholamine solution is 20-40% by weight.

[0024] Preferably, in step S1, the amount of the catalyst used is 0.1-0.3 wt % based on the total weight of the carbon dioxide absorbing liquid.

[0025] Preferably, the carbon dioxide content in the carbon dioxide mixed gas is 11-15% by volume.

[0026] Compared with the prior art, the present invention has at least the following advantages: (1) The method of the present invention comprises mixing urea, nickel salt, aluminum salt and a mixed solvent containing organic matter simultaneously by ultrasonic means, and the mixed solution is subjected to a hydrothermal reaction, and the obtained product is calcined at a high temperature, so as to prepare a nanosheet hydrotalcite catalyst having a large specific surface area, a large number of active sites, a high activity and a stable structure at a high temperature, which promotes the absorption of carbon dioxide by alcoholamine.

[0027] (2) The preparation process of the method described in the present invention is simple and uses fewer types of raw materials. It only requires ultrasonic mixing of urea, nickel salt, aluminum salt and mixed solvent, followed by hydrothermal reaction and calcination to prepare the nanosheet hydrotalcite catalyst.

[0028] (3) The nanosheet hydrotalcite catalyst provided by the present invention is used to catalyze the absorption of carbon dioxide by alcohol amine solution, and can significantly improve the absorption rate and absorption performance of carbon dioxide compared with existing catalysts. Specifically, the nanosheet hydrotalcite catalyst has unique physical and chemical properties, and exhibits the following technical advantages in the process of promoting the absorption of carbon dioxide by alcohol amines: First, the hydrotalcite catalyst has an extremely high specific surface area, and more active sites can be used for catalytic reactions, thereby increasing the contact frequency and reaction rate between alcohol amines and carbon dioxide. Second, the hydrotalcite catalyst has good dispersibility in the solution, which helps the alcohol amine molecules to be more evenly distributed on the catalyst surface, thereby improving the absorption efficiency. Third, the thin layer structure of the nanosheet hydrotalcite catalyst facilitates rapid mass transfer between gas and liquid, reduces mass transfer resistance, and increases the absorption rate of carbon dioxide. In short, the nanosheet hydrotalcite catalyst of the present invention has many technical advantages in the process of promoting the absorption of carbon dioxide by alcohol amines, and these advantages can make it a hot material for improving carbon dioxide capture efficiency and research. DETAILED DESCRIPTION

[0029] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0030] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0031] The method for preparing the nanosheet hydrotalcite catalyst provided by the present invention comprises the following steps: (1) mixing urea, nickel salt, aluminum salt and a mixed solvent under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains an organic solvent and water; (2) subjecting the mixed solution to a hydrothermal reaction, and then calcining the obtained reaction product.

[0032] In the method described in the present invention, urea, nickel salt, aluminum salt and a mixed solvent containing organic matter are simultaneously mixed by ultrasonic means, so that the dispersion of urea, nickel salt and aluminum salt in the mixed solution can be greatly improved. After the mixed solution is subjected to a hydrothermal reaction, the obtained layered nickel-aluminum hydrotalcite product is calcined at a high temperature, so that a binary nickel-aluminum hydrotalcite in the form of nanosheets with a large specific surface area, many active sites and high activity can be prepared. The nickel-aluminum hydrotalcite is calcined at a high temperature during the preparation process, so its structure is very stable.

[0033] In the present invention, the mixed solvent needs to use specific alcohol amines and / or alcohols to significantly increase the specific surface area of ​​the prepared hydrotalcite catalyst and > 200m 2 / g, so that the prepared nanosheet hydrotalcite catalyst has a high absorption efficiency for carbon dioxide. In a more preferred embodiment, the organic solvent in step (1) is selected from at least one of ethanolamine, N-methyldiethanolamine, n-hexadecanol and n-hexanol.

[0034] In some embodiments, the volume ratio of the water to the organic solvent in the mixed solvent may be 2-6: 1, such as 2: 1, 2.5: 1, 3: 1, 3.5: 1, 4: 1, 4.5: 1, 5: 1, 5.5: 1 or 6: 1. In the present invention, the volume ratio of the water to the organic solvent is limited to this range, which can reduce the volatilization of the absorption solution and realize the long-term stable operation of the large-scale carbon capture device.

[0035] In the present invention, in order to further improve the dispersion of the raw materials in the mixed solution, thereby promoting the uniform growth of hydrotalcite crystals and improving the regularity of its structure; through ultrasound-assisted synthesis, hydrotalcite with higher crystallinity, smaller particle size and larger specific surface area can be obtained. The ultrasonic conditions in step (1) can be optimized. In some preferred embodiments, the ultrasonic conditions in step (1) include: the ultrasonic frequency is 80-120kHz, such as 80kHz, 90kHz, 100kHz, 110kHz or 120kHz; the ultrasonic power is 500-700W, such as 500W, 550W, 600W, 650W or 700W; the ultrasonic time is 5-15min, such as 5min, 10min or 15min.

[0036] In some embodiments, in step (1), based on 1000 mL of the mixed solvent, the amount of urea used can be 0.1-2 mol, for example, 0.1 mol, 0.5 mol, 0.8 mol, 1 mol, 1.2 mol, 1.5 mol, 1.8 mol or 2 mol.

[0037] In the method of the present invention, in order to prepare nickel-aluminum nanosheet hydrotalcite, in step (1), the usage ratio of the urea, the nickel salt and the aluminum salt can be determined in a conventional manner. In some embodiments, the nickel salt is calculated as Ni, the aluminum salt is calculated as Al, and the molar ratio of the usage of the urea, the nickel salt and the aluminum salt can be 5-30:2-4:1.

[0038] In the present invention, the nickel salt may be a conventional choice in the art. In some embodiments, the nickel salt may be selected from at least one of nickel nitrate, nickel chloride and nickel sulfate. In the present invention, the aluminum salt may be a conventional choice in the art. In other embodiments, the aluminum salt may be selected from at least one of aluminum nitrate, aluminum chloride and aluminum sulfate.

[0039] In some preferred embodiments, the temperature of the hydrothermal reaction in step (2) is 130-200°C, for example, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C; and the time is 4-8h, for example, 4h, 4.5h, 5h, 5.5h, 6h, 6.6h, 7h, 7.5h or 8h.

[0040] In order to obtain nano-sheet-shaped nickel-aluminum hydrotalcite and simultaneously increase the specific surface area and active sites of the hydrotalcite catalyst, in a preferred embodiment, the calcination temperature in step (2) is 400-600° C. and the calcination time is 2-5 h.

[0041] In the method described in the present invention, the operation process of step (2) includes: subjecting the mixed solution to a hydrothermal reaction, filtering after the reaction is completed, and washing and drying the obtained reaction product, and then calcining it.

[0042] The method disclosed in the invention has a simple preparation process and uses fewer types of raw materials. It only requires ultrasonic mixing of urea, nickel salt, aluminum salt and a mixed solvent followed by hydrothermal reaction and calcination to prepare the nanosheet hydrotalcite catalyst.

[0043] The present invention also provides a nanosheet hydrotalcite catalyst prepared by the method described above. The nanosheet hydrotalcite catalyst provided by the present invention has a large specific surface area, many active sites, high activity, and a stable structure at high temperatures. In some embodiments, the specific surface area of ​​the nanosheet hydrotalcite catalyst can be 216-258 m 2 / g.

[0044] The present invention also provides the use of the nanosheet hydrotalcite catalyst prepared by the method described above or the nanosheet hydrotalcite catalyst described above in catalyzing the absorption of carbon dioxide by an alcoholamine solution.

[0045] The inventors found that hydrotalcite plays an important role in promoting the absorption of carbon dioxide by alcohol amine solution, mainly in the following aspects: (1) Acid-base neutralization reaction: The structure of hydrotalcite consists of two layers of hydroxide plates and guest water molecules and anions between the plates. These hydroxide plates are alkaline and can undergo acid-base neutralization reaction with carbon dioxide to generate carbonate or bicarbonate ions. This process can reduce the partial pressure of carbon dioxide in the solution, thereby promoting the reaction of alcoholamine with carbon dioxide; (2) Providing active sites: The layered structure of hydrotalcite provides a large number of active sites, which can promote the interaction between olamines and carbon dioxide. The metal ions (such as nickel, aluminum, etc.) in hydrotalcite can act as Lewis acids and interact with the basic oxygen atoms in the carbon dioxide molecules, thereby activating the carbon dioxide molecules and making them more likely to react with olamines; (3) Catalytic effect: Hydrotalcite can act as a catalyst to accelerate the reaction rate of alcohol amine and carbon dioxide. Its catalytic effect may be due to the fact that the metal ions in hydrotalcite can reduce the activation energy of the reaction, thereby increasing the reaction rate; (4) Improve the dispersibility of alcohol amines: Hydrotalcite can be used as a carrier to improve the dispersibility of alcohol amines in the solution. Good dispersibility helps to increase the contact area between alcohol amines and carbon dioxide, thereby improving the absorption efficiency; (5) Stabilizing the alcoholamine solution: The presence of hydrotalcite can inhibit the degradation of alcoholamine and improve the stability of the alcoholamine solution. This helps to maintain the absorption performance of the alcoholamine and extend its service life; (6) Promote the desorption of carbon dioxide: During the carbon dioxide absorption process, hydrotalcite can also promote the desorption of carbon dioxide. When the absorption is saturated, by changing the conditions (such as increasing the temperature, reducing the pressure or changing the pH value), hydrotalcite can help release the absorbed carbon dioxide and achieve the regeneration of the alcohol amine.

[0046] In addition, since the nano-sheet hydrotalcite catalyst prepared by the present invention has unique physical and chemical properties, it also exhibits the following technical advantages in the process of promoting the absorption of carbon dioxide by alcohol amines: first, the nano-sheet hydrotalcite catalyst has an extremely high specific surface area, and more active sites can be used for catalytic reaction, thereby increasing the contact frequency and reaction rate between alcohol amines and carbon dioxide. Second, the nano-sheet hydrotalcite catalyst has good dispersibility in the solution, which helps the alcohol amine molecules to be more evenly distributed on the catalyst surface, thereby improving the absorption efficiency. Third, the thin layer structure of the nano-sheet hydrotalcite catalyst helps the rapid mass transfer between gas and liquid, reduces the mass transfer resistance, and increases the absorption rate of carbon dioxide.

[0047] The present invention also provides a method for absorbing carbon dioxide, which comprises the following steps: S1, mixing the alcohol amine solution with the catalyst to obtain a carbon dioxide absorption liquid; S2, contacting the carbon dioxide absorbing liquid with the carbon dioxide mixed gas at 30-50° C. and normal pressure to absorb carbon dioxide in the carbon dioxide mixed gas; S3, after the absorption is completed, the carbon dioxide absorption liquid is desorbed at 90-115° C. and normal pressure; Wherein, the catalyst is the nanosheet hydrotalcite catalyst prepared by the method described above or the nanosheet hydrotalcite catalyst described above.

[0048] In the present invention, the nanosheet hydrotalcite catalyst has an extremely high specific surface area, more active sites, high absorption efficiency and selectivity, and because the nanosheet hydrotalcite catalyst is calcined at high temperature during the preparation process, the nanosheet hydrotalcite catalyst can maintain structural stability; because the nanosheet hydrotalcite catalyst can promote the desorption of carbon dioxide during the regeneration process of alcohol amines, energy consumption can be reduced.

[0049] In some embodiments, in step S1, the alcoholamine compound in the alcoholamine solution is selected from at least two of ethanolamine, N-methyldiethanolamine and 2-amino-2-methyl-1-propanol.

[0050] In some embodiments, in step S1, the concentration of the alcoholamine solution may be 20-40 wt %.

[0051] In some embodiments, in step S1, the amount of the catalyst used may be 0.1-0.3 wt % based on the total weight of the carbon dioxide absorbing liquid.

[0052] In some embodiments, the carbon dioxide content in the carbon dioxide mixed gas is 11-15% by volume. In addition to carbon dioxide, the carbon dioxide mixed gas also contains gases such as nitrogen.

[0053] The present invention focuses on solving the problems of reduced structure or activity when using hydrotalcite catalysts, and develops more stable catalyst materials and synthesis methods by improving the types of hydrotalcite, optimizing the design of the catalyst, and improving the absorption efficiency and selectivity.

[0054] The following examples further illustrate the preparation method of the nanosheet hydrotalcite catalyst of the present invention and its application in the absorption of carbon dioxide by an alcohol amine solution. The examples are implemented based on the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples.

[0055] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.

[0056] Example 1 (1) Urea, nickel salt (nickel nitrate), aluminum salt (aluminum nitrate) and a mixed solvent are mixed under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains water and ethanolamine in a volume ratio of 2:1; based on 1000 mL of the mixed solvent, the amount of urea is 0.5 mol; the molar ratio of the urea, the nickel salt (calculated as nickel element) and the aluminum salt (calculated as aluminum element) is 15:3:1; the frequency of the ultrasound is 100 kHz, the power of the ultrasound is 500 W, and the time of the ultrasound is 15 min; (2) The mixed solution was hydrothermally reacted at 150° C. for 4 h, filtered, and then the obtained solid phase product was washed and dried, and then calcined at 600° C. for 4 h.

[0057] Example 2 (1) Urea, nickel salt (nickel sulfate), aluminum salt (aluminum sulfate) and a mixed solvent are mixed under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains water and N-methyldiethanolamine in a volume ratio of 6:1; based on 1000 mL of the mixed solvent, the amount of urea is 1.5 mol; the molar ratio of the urea, the nickel salt (calculated as nickel element) and the aluminum salt (calculated as aluminum element) is 30:4:1; the frequency of the ultrasound is 120 kHz, the power of the ultrasound is 700 W, and the time of the ultrasound is 5 min; (2) The mixed solution was hydrothermally reacted at 200° C. for 8 h, filtered, and then the obtained solid phase product was washed and dried, and then calcined at 500° C. for 4 h.

[0058] Example 3 (1) Urea, nickel salt (nickel nitrate), aluminum salt (aluminum nitrate) and a mixed solvent are mixed under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains water and ethanolamine in a volume ratio of 4:1; based on 1000 mL of the mixed solvent, the amount of urea is 2 mol, and the molar ratio of the amount of the urea, the nickel salt (calculated as nickel element) and the aluminum salt (calculated as aluminum element) is 5:2:1; the frequency of the ultrasound is 80 kHz, the power of the ultrasound is 600 W, and the time of the ultrasound is 10 min; (2) The mixed solution was hydrothermally reacted at 180° C. for 6 h, filtered, and then the obtained solid phase product was washed and dried, and then calcined at 400° C. for 4 h.

[0059] Example 4 (1) Urea, nickel salt (nickel sulfate), aluminum salt (aluminum sulfate) and a mixed solvent are mixed under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains water and ethanolamine in a volume ratio of 4:1; based on 1000 mL of the mixed solvent, the amount of urea is 1 mol; the molar ratio of the urea, the nickel salt (calculated as nickel element) and the aluminum salt (calculated as aluminum element) is 15:4:1; the frequency of the ultrasound is 100 kHz, the power of the ultrasound is 600 W, and the time of the ultrasound is 10 min; (2) The mixed solution was hydrothermally reacted at 165° C. for 6 h, filtered, and then the obtained solid phase product was washed and dried, and then calcined at 500° C. for 2 h.

[0060] Comparative Example 1 The method of Example 1 is followed, except that in step (1), no ultrasound is performed and the mixture is directly stirred and mixed.

[0061] The specific operation process is as follows: (1) urea, nickel salt (nickel nitrate), aluminum salt (aluminum nitrate) and a mixed solvent are mixed under stirring conditions to obtain a mixed solution, wherein the mixed solvent contains water and ethanolamine in a volume ratio of 2:1; based on 1000 mL of the mixed solvent, the amount of urea is 0.5 mol; the molar ratio of the urea, the nickel salt (calculated as nickel element) and the aluminum salt (calculated as aluminum element) is 15:3:1; the stirring rate is 200 revolutions per minute, and the stirring time is 15 minutes; (2) The mixed solution was hydrothermally reacted at 150° C. for 4 h, filtered, and then the obtained solid phase product was washed and dried, and then calcined at 600° C. for 4 h.

[0062] Comparative Example 2 The method of Example 1 was followed, except that water was used as the solvent.

[0063] The specific operation process is as follows: (1) Urea, nickel salt (nickel nitrate), aluminum salt (aluminum nitrate) and solvent (water) are mixed under ultrasonic conditions to obtain a mixed solution, wherein the amount of urea is 0.5 mol based on 1000 mL of water; the molar ratio of the urea, the nickel salt (calculated as nickel element) and the aluminum salt (calculated as aluminum element) is 15:3:1; the ultrasonic frequency is 100 kHz, the ultrasonic power is 500 W, and the ultrasonic time is 15 min; (2) The mixed solution was hydrothermally reacted at 150° C. for 4 h, filtered, and then the obtained solid phase product was washed and dried, and then calcined at 600° C. for 4 h.

[0064] Comparative Example 3 The method of Example 1 was followed, except that the ethanolamine in the mixed solvent was replaced by n-hexanol.

[0065] The specific operation process is as follows: (1) Urea, a nickel salt (nickel nitrate), an aluminum salt (aluminum nitrate) and a mixed solvent are mixed under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains water and hexanol in a volume ratio of 2:1; based on 1000 mL of the mixed solvent, the amount of urea is 0.5 mol; the molar ratio of the urea, the nickel salt (calculated as nickel element) and the aluminum salt (calculated as aluminum element) is 15:3:1; the frequency of the ultrasound is 100 kHz, the power of the ultrasound is 500 W, and the time of the ultrasound is 15 min; (2) The mixed solution was hydrothermally reacted at 150° C. for 4 h, filtered, and then the obtained solid phase product was washed and dried, and then calcined at 600° C. for 4 h.

[0066] Comparative Example 4 The method of Example 1 is followed, except that in step (2), no calcination is performed.

[0067] The specific operation process is as follows: (1) Urea, nickel salt (nickel nitrate), aluminum salt (aluminum nitrate) and a mixed solvent are mixed under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains ethanolamine and water in a volume ratio of 2:1; based on 1000 mL of the mixed solvent, the amount of urea is 0.5 mol; the molar ratio of the urea, the nickel salt (calculated as nickel element) and the aluminum salt (calculated as aluminum element) is 15:3:1; the frequency of the ultrasound is 100 kHz, the power of the ultrasound is 500 W, and the time of the ultrasound is 15 min; (2) The mixed solution is subjected to a hydrothermal reaction at 150° C. for 4 h, filtered, and then the obtained solid phase product is washed and dried.

[0068] Test Example 1 The specific surface areas of the products prepared in the examples and comparative examples were measured using BET. The results are shown in Table 1.

[0069] Table 1

[0070] It can be seen from the results in Table 1 that, compared with the comparative example, the specific surface area of ​​the hydrotalcite catalyst prepared by the method of the embodiment of the present invention is significantly increased, and is greater than 200m 2 / g.

[0071] Test Example 2 S1. The products prepared in the embodiment and the comparative example are mixed as catalysts with an alcohol amine solution (the alcohol amine solution contains ethanolamine and N-methyldiethanolamine, wherein the concentration of ethanolamine is 10% by weight and the concentration of N-methyldiethanolamine is 20% by weight) to obtain a carbon dioxide absorption liquid, wherein the amount of the catalyst is 0.2% by weight of the carbon dioxide absorption liquid; S2, contacting 100 g of carbon dioxide absorption liquid with a carbon dioxide mixed gas at 35° C. and normal pressure, absorbing carbon dioxide in the carbon dioxide mixed gas until absorption is saturated, wherein the carbon dioxide content in the carbon dioxide mixed gas is 13% by volume, and the remainder is nitrogen; S3. After the absorption is saturated, the carbon dioxide absorption liquid is desorbed at 110° C. and normal pressure.

[0072] The absorption rate and desorption rate of the carbon dioxide absorption liquid obtained by mixing the products prepared in the examples and comparative examples as catalysts with ethanolamine solutions were calculated, and the results are shown in Table 2.

[0073] Table 2

[0074] It can be seen from the results in Table 2 that, compared with the comparative example, the nanosheet hydrotalcite prepared by the method of the embodiment of the present invention as a catalyst can improve the absorption efficiency of carbon dioxide by the alcoholamine solution, and the desorption rate is relatively high.

[0075] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a nanosheet hydrotalcite catalyst, characterized in that: The method comprises the following steps: (1) mixing urea, nickel salt, aluminum salt and a mixed solvent under ultrasonic conditions to obtain a mixed solution, wherein the mixed solvent contains an organic solvent and water, and the organic solvent is selected from at least one of ethanolamine, N-methyldiethanolamine, n-hexadecanol and n-hexanol; (2) subjecting the mixed solution to a hydrothermal reaction, and then calcining the obtained reaction product.

2. The method according to claim 1, characterized in that In the mixed solvent, the volume ratio of the water to the organic solvent is 2-6.

3. The method according to claim 1 or 2, characterized in that: In step (1), the ultrasonic conditions include: the ultrasonic frequency is 80-120 kHz, the ultrasonic power is 500-700 W, and the ultrasonic time is 5-15 min.

4. The method according to any one of claims 1 to 3, characterized in that: In step (1), the amount of urea used is 0.1-2 mol based on 1000 mL of the mixed solvent.

5. The method according to any one of claims 1 to 4, characterized in that: In step (1), the nickel salt is calculated as Ni, the aluminum salt is calculated as Al, and the molar ratio of the urea, the nickel salt and the aluminum salt is 5-30:2-4:1; Preferably, the nickel salt is selected from at least one of nickel nitrate, nickel chloride and nickel sulfate; Preferably, the aluminum salt is selected from at least one of aluminum nitrate, aluminum chloride and aluminum sulfate.

6. The method according to any one of claims 1 to 5, characterized in that: In step (2), the conditions of the hydrothermal reaction include: temperature of 130-200° C. and time of 4-8 h.

7. The method according to any one of claims 1 to 6, characterized in that: In step (2), the calcination conditions include: temperature of 400-600°C and time of 2-5 h.

8. A nanosheet hydrotalcite catalyst prepared by the method according to any one of claims 1 to 7; Preferably, the specific surface area of ​​the nanosheet hydrotalcite catalyst is 216-258 m 2 / g.

9. Use of the nanosheet hydrotalcite catalyst prepared by the method according to any one of claims 1 to 7 or the nanosheet hydrotalcite catalyst according to claim 8 in absorbing carbon dioxide with an alcoholamine solution.

10. A method for absorbing carbon dioxide, characterized in that: The method comprises the following steps: S1, mixing the alcohol amine solution with the catalyst to obtain a carbon dioxide absorption liquid; S2, contacting the carbon dioxide absorbing liquid with the carbon dioxide mixed gas at 30-50° C. and normal pressure to absorb carbon dioxide in the carbon dioxide mixed gas; S3, after the absorption is completed, the carbon dioxide absorption liquid is desorbed at 90-115° C. and normal pressure; Wherein, the catalyst is a nanosheet hydrotalcite catalyst prepared by the method according to any one of claims 1 to 7 or a nanosheet hydrotalcite catalyst according to claim 8.

11. The method according to claim 10, characterized in that In step S1, the alcoholamine compound in the alcoholamine solution is selected from at least two of ethanolamine, N-methyldiethanolamine and 2-amino-2-methyl-1-propanol; Preferably, in step S1, the concentration of the alcoholamine solution is 20-40% by weight; Preferably, in step S1, the amount of the catalyst is 0.1-0.3% by weight based on the total weight of the carbon dioxide absorbing liquid; Preferably, the carbon dioxide content in the carbon dioxide mixed gas is 11-15% by volume.