Catalyst as well as preparation method and application thereof

Through the catalyst supported by nickel nanoparticles and the hydrogenation process of continuous drip fixed bed, the existing catalysts have solved the problem of low efficiency and high cost in the preparation of succinic anhydride in a continuous drip bed, and achieved efficient and stable succinic anhydride Production.

CN119075991APending Publication Date: 2024-12-06TAN KAH KEE INNOVATION LAB +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411371889.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing catalysts are difficult to effectively prepare succinic anhydride in continuous drip bed hydrogenation process, and the cost is high, especially high-performance and high-stability forming catalysts, which are insufficiently used in this process.

Method used

A catalyst supported by a carrier-loaded nickel nanoparticles is prepared by precipitation method, combined with a continuous drip fixed bed hydrogenation process, to achieve efficient preparation and stability improvement of the catalyst.

Benefits of technology

Under mild reaction conditions, the 100% conversion rate and 99.9% selectivity of maleic anhydride are achieved, and the catalyst stability can reach more than 200 hours, which reduces the process cost and is suitable for the continuous production of succinic anhydride.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075991A_ABST
    Figure CN119075991A_ABST
Patent Text Reader

Abstract

The invention provides a catalyst as well as a preparation method and application thereof, and relates to the technical field of catalysts. The catalyst comprises a carrier and a metal nickel-based active component, wherein the metal nickel-based active component is nickel nanoparticles loaded on the carrier. Through verification, when the catalyst is applied to a continuous trickle fixed bed reaction device for hydrogenation reduction reaction, the catalyst has excellent activity and selectivity for catalyzing maleic anhydride hydrogenation to prepare butanedioic anhydride, the highest maleic anhydride conversion rate can reach 100% under the mild reaction conditions that the air speed is 1.0 h <-1 >, the temperature is 120 DEG C and the pressure is 0.5 MPa H2, and the selectivity is 99.9%; meanwhile, the catalyst can stably run for more than 200 hours, has excellent catalytic stability and is expected to be applied to industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a catalyst and a preparation method and application thereof. Background Art

[0002] Succinic anhydride is an important organic synthesis intermediate and fine chemical raw material, which is widely used in medicine, pesticides, dyes and other fields. As an important chemical raw material and intermediate for the synthesis of biodegradable plastic polybutylene succinate (PBS), the demand for succinic anhydride is increasing with the continuous expansion of PBS production capacity in my country. With the maturity of the process route for the preparation of succinic anhydride by oxidation of n-butane, the raw material maleic anhydride has an abundant source and is cheap. The hydrogenation of maleic anhydride to succinic anhydride has great economic benefits and is expected to become the mainstream technology for the industrial preparation of succinic anhydride.

[0003] The continuous fixed bed hydrogenation is a widely used gas-liquid-solid three-phase reactor, especially in the process of oil refining and oil processing. Compared with intermittent reactors, the fixed bed hydrogenation continuous trickle bed can effectively improve the conversion rate, avoid by-product interference, reduce the reaction heat effect to ensure process safety, and at the same time, the device occupies a smaller space to achieve continuous production of larger quantities of products, ensuring economic efficiency. Therefore, the development of high-performance and high-stability formed catalysts and the use of continuous trickle fixed bed hydrogenation process for the hydrogenation of maleic anhydride to succinic anhydride is of great significance to the development of chemical industry.

[0004] Chinese patent CN116037134A discloses a mixed catalyst with NiO / SnO2 / CeO2 as active component, adopts slurry bed catalytic process, uses 1.6wt% catalyst dosage, reacts 2h at 80℃, 2.5MPa H2 atmosphere, and the yield of succinic anhydride reaches 99.7%; Chinese patent CN102229587A discloses a method for catalytic hydrogenation of maleic anhydride to succinic anhydride by nano-nickel, adopts autoclave intermittent reaction process, uses only 1wt% catalyst dosage of nickel-based nano-material, takes acetic anhydride as solvent, reacts 4h at 80℃, 2.5MPa H2 atmosphere, and the yield of succinic anhydride reaches more than 98%. Although the above-mentioned catalyst dosage is small, it has high activity, high selectivity and high yield to produce succinic anhydride, but it is not suitable for continuous trickle bed hydrogenation process, and it cannot be continuously produced in practice.

[0005] Chinese patent CN105597742A discloses a molded Pd-based catalyst for use in hydrogenation of maleic anhydride to produce succinic anhydride. Although the patent uses a continuous trickle bed reactor and the catalyst has a high maleic anhydride mass space velocity, the process has a large molar ratio of hydrogen anhydride (100) and uses the precious metal palladium, resulting in high catalyst cost. Therefore, it is crucial to develop a low-cost, high-activity molded nickel-based catalyst for use in the continuous hydrogenation of maleic anhydride to succinic anhydride.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The first object of the present invention is to provide a catalyst having excellent activity and selectivity for catalyzing the hydrogenation of maleic anhydride to prepare succinic anhydride.

[0008] The second object of the present invention is to provide a method for preparing a catalyst.

[0009] The third object of the present invention is to provide a use of the catalyst as a catalyst for preparing succinic anhydride by hydrogenation reduction.

[0010] The fourth object of the present invention is to provide a method for preparing succinic anhydride, wherein the catalyst is applied to a continuous trickle fixed bed hydrogenation process, which has the advantages of low reaction temperature and low hydrogen pressure; at the same time, the catalyst has good stability during the synthesis process and can be stably circulated for more than 200 hours, which is beneficial to reducing process costs.

[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0012] In a first aspect, the present invention provides a catalyst, comprising a carrier and a metal nickel-based active component, wherein the metal nickel-based active component is nickel nanoparticles supported on the carrier.

[0013] Furthermore, the carrier includes one of alumina beads, silica beads, titanium dioxide beads or shaped carbon chips.

[0014] Preferably, the particle size of the carrier is 0.05 to 5 mm, preferably 0.5 to 2.0 mm.

[0015] Furthermore, the molded carbon crumbs are obtained by mixing activated carbon powder with a strengthening agent, a binder, and a pore-forming agent, and then extruding and molding the mixture.

[0016] Furthermore, the reinforcing agent includes any one of glass fiber, aluminum oxide or silicon oxide, or a combination of at least two thereof.

[0017] Furthermore, the binder includes any one of hydroxypropyl cellulose, hydroxymethyl cellulose, polyvinyl alcohol, gum, sesbania powder, aluminum sol or silica sol, or a combination of at least two thereof.

[0018] Furthermore, the pore-forming agent includes any one of dry starch, polyethylene glycol, polyethylene oxide, paraffin or glycerol, or a combination of at least two thereof.

[0019] Furthermore, the 2p 3 / 2 orbital binding energy of the nickel element in the nickel nanoparticles is 849 eV to 868 eV.

[0020] In a second aspect, the present invention provides a method for preparing the catalyst as described in the first aspect, the preparation method comprising:

[0021] (A) adding a carrier to a metal nickel salt solution and mixing, then adding an alkaline precipitant to precipitate the metal nickel salt onto the carrier, and drying to obtain a precursor A;

[0022] (B) Under reducing atmosphere conditions, the precursor A is calcined and reduced to obtain the catalyst.

[0023] Furthermore, the metal nickel salt in the metal nickel salt solution of step (A) includes any one of nickel chloride, nickel nitrate, nickel acetate, nickel formate or nickel acetylacetonate, or a combination of at least two thereof.

[0024] Furthermore, the solvent in the metal nickel salt solution in step (A) includes at least one of water, methanol, ethanol, tetrahydrofuran or N,N-dimethylformamide.

[0025] Furthermore, the alkaline precipitant in step (A) includes any one of ammonia solution, alkali metal hydroxide or alkali metal carbonate, or a combination of at least two of them.

[0026] Furthermore, the ammonia solution is aqueous ammonia and / or ammonia in methanol solution.

[0027] Furthermore, the alkali metal hydroxide includes sodium hydroxide and / or potassium hydroxide.

[0028] Furthermore, the alkali metal carbonate includes sodium carbonate and / or potassium carbonate.

[0029] Furthermore, the reducing atmosphere in step (B) includes any one of hydrogen, hydrogen / argon mixed gas, carbon monoxide, methane or acetylene, or a combination of at least two thereof.

[0030] Furthermore, the temperature of the calcination reduction in step (B) is 100-600°C.

[0031] Furthermore, the calcination reduction time in step (B) is 1 to 12 hours.

[0032] In a third aspect, the present invention provides a use of the catalyst as described in the first aspect, or the catalyst prepared by the preparation method as described in the second aspect, as a catalyst for preparing succinic anhydride by hydrogenation reduction.

[0033] In a fourth aspect, the present invention provides a method for preparing succinic anhydride, the preparation method comprising:

[0034] In the presence of the catalyst as described in the first aspect or the catalyst prepared by the preparation method as described in the second aspect, maleic anhydride is subjected to a hydrogenation reduction reaction to obtain succinic anhydride.

[0035] Furthermore, the preparation method of succinic anhydride specifically comprises the following steps:

[0036] (I) placing the above catalyst in a continuous trickle fixed bed reaction device;

[0037] (II) Maleic anhydride is placed in a solvent and mixed to obtain a reaction solution, and the reaction solution is injected into a continuous trickle fixed bed reactor under a reducing gas atmosphere to carry out a hydrogenation reduction reaction to obtain succinic anhydride.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) The catalyst provided by the present invention comprises a carrier and a metal nickel-based active component, wherein the metal nickel-based active component is nickel nanoparticles supported on the carrier. It has been verified that the catalyst of the present application is applied to a continuous trickle fixed bed reactor for hydrogenation reduction reaction, and has excellent activity and selectivity for catalyzing the hydrogenation of maleic anhydride to prepare succinic anhydride. -1 Under mild reaction conditions of 120°C and 0.5MPa H2, the maleic anhydride conversion rate was 100% and the selectivity was 99.9%.

[0040] (2) The preparation method of the catalyst provided by the present invention comprises first adding a carrier to a metal nickel salt solution and mixing, then adding an alkaline precipitant to precipitate the metal nickel salt onto the carrier and drying to obtain a precursor A; then, under a reducing atmosphere, the precursor A is calcined and reduced to obtain the catalyst of the present application. The catalyst prepared by the precipitation method of the present application has the technical advantages of simple preparation process, low production cost, and being conducive to large-scale production.

[0041] (3) The hydrogenation synthesis method of succinic anhydride provided by the present invention, the method first places the above-mentioned catalyst in a continuous trickle fixed bed reaction device, and then injects the maleic anhydride reaction solution into the continuous trickle fixed bed reaction device under a reducing gas atmosphere for hydrogenation reduction reaction to obtain succinic anhydride. The hydrogenation synthesis method of the present application adopts a continuous trickle fixed bed hydrogenation process, which has the advantages of low reaction temperature and low hydrogen pressure, and can realize continuous production of succinic anhydride under mild conditions. At the same time, the catalyst has good stability during the synthesis process and can be stably circulated for more than 200 hours, which is beneficial to reduce the process cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0043] Figure 1 This is a scanning electron microscope characterization image of the Ni / C-TR catalyst obtained in Example 5 of the present invention;

[0044] Figure 2 This is the XRD characterization diagram of the Ni / C-TR catalyst obtained in Example 5 of the present invention;

[0045] Figure 3 This is the XPS characterization diagram of the Ni / C-TR catalyst obtained in Example 5 of the present invention;

[0046] Figure 4 This is a graph showing the stability test of maleic anhydride hydrogenation of the Ni / C-TR catalyst obtained in Example 5 of the present invention. DETAILED DESCRIPTION

[0047] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] According to one aspect of the present invention, a catalyst comprises a carrier and a metal nickel-based active component, wherein the metal nickel-based active component is nickel nanoparticles supported on the carrier.

[0049] The catalyst provided by the present invention comprises a carrier and a metal nickel-based active component, wherein the metal nickel-based active component is nickel nanoparticles supported on the carrier. It has been verified that the catalyst of the present application is applied to a continuous trickle fixed bed reactor for hydrogenation reduction reaction, and has excellent activity and selectivity for catalyzing the hydrogenation of maleic anhydride to prepare succinic anhydride. -1 Under mild reaction conditions of 120°C and 0.5MPa H2, the maleic anhydride conversion rate was 100% and the selectivity was 99.9%.

[0050] In a preferred embodiment of the present invention, the carrier is a shaped carrier, and the shaped carrier includes one of alumina beads, silica beads, titanium dioxide beads or shaped carbon chips.

[0051] In a preferred embodiment of the present invention, the molded carbon crumbs are obtained by mixing activated carbon powder with a strengthening agent, a binder, and a pore-forming agent and then extruding the mixture.

[0052] In a preferred embodiment of the present invention, the reinforcing agent comprises any one of glass fiber, aluminum oxide or silicon oxide, or a combination of at least two thereof.

[0053] In a preferred embodiment of the present invention, the binder includes any one of hydroxypropyl cellulose, hydroxymethyl cellulose, polyvinyl alcohol, gum, sesbania powder, aluminum sol or silica sol, or a combination of at least two thereof.

[0054] In a preferred embodiment of the present invention, the pore-forming agent comprises any one of dry starch, polyethylene glycol, polyethylene oxide, paraffin or glycerol, or a combination of at least two thereof.

[0055] In a preferred embodiment of the present invention, the 2p 3 / 2 orbital binding energy of nickel element in the nickel nanoparticles is 849 eV to 868 eV.

[0056] According to one aspect of the present invention, a method for preparing the above-mentioned catalyst comprises:

[0057] (A) adding a carrier to a metal nickel salt solution and mixing, then adding an alkaline precipitant to precipitate the metal nickel salt onto the carrier, and drying to obtain a precursor A;

[0058] (B) Under reducing atmosphere conditions, the precursor A is calcined and reduced to obtain the catalyst.

[0059] The preparation method of the catalyst provided by the present invention first adds a carrier to a metal nickel salt solution and mixes, then adds an alkaline precipitant to precipitate the metal nickel salt on the carrier and dry to obtain a precursor A; then, under a reducing atmosphere, the precursor A is calcined and reduced to obtain the catalyst of the present application. The catalyst prepared by the development precipitation method of the present application has the technical advantages of simple preparation process, low production cost, and conducive to large-scale production.

[0060] In a preferred embodiment of the present invention, the metal nickel salt in the metal nickel salt solution of step (A) comprises any one of nickel chloride, nickel nitrate, nickel acetate, nickel formate or nickel acetylacetonate, or a combination of at least two thereof.

[0061] In a preferred embodiment of the present invention, the solvent in the metal nickel salt solution in step (A) comprises any one of water, methanol, ethanol, tetrahydrofuran or N,N-dimethylformamide, or a combination of at least two thereof.

[0062] In a preferred embodiment of the present invention, the alkaline precipitant in step (A) comprises any one of ammonia solution, alkali metal hydroxide or alkali metal carbonate, or a combination of at least two thereof.

[0063] In a preferred embodiment of the present invention, the ammonia solution is aqueous ammonia.

[0064] In a preferred embodiment of the present invention, the alkali metal hydroxide includes sodium hydroxide and / or potassium hydroxide.

[0065] In a preferred embodiment of the present invention, the alkali metal carbonate includes sodium carbonate and / or potassium carbonate.

[0066] In a preferred embodiment of the present invention, the reducing atmosphere in step (B) comprises any one of hydrogen, hydrogen / argon mixed gas, carbon monoxide, methane or acetylene, or a combination of at least two thereof.

[0067] Preferably, the volume percentage of hydrogen in the hydrogen / argon mixture is 5% to 100%, for example, it can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0068] In a preferred embodiment of the present invention, the temperature of the calcination reduction in step (B) is 100-600°C, for example, it can be 100°C, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, etc.

[0069] In a preferred embodiment of the present invention, the calcination reduction time in step (B) is 1 to 12 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, etc.

[0070] According to one aspect of the present invention, the present invention provides a use of the catalyst as described in the first aspect, or the catalyst prepared by the preparation method as described in the second aspect as a catalyst for preparing succinic anhydride by hydrogenation reduction.

[0071] According to one aspect of the present invention, the present invention provides a method for preparing succinic anhydride, the preparation method comprising:

[0072] In the presence of the catalyst as described above, or the catalyst prepared by the preparation method as described above, maleic anhydride is subjected to hydrogenation reduction reaction to obtain succinic anhydride.

[0073] In a preferred embodiment of the present invention, the preparation method of succinic anhydride specifically comprises the following steps:

[0074] (I) placing the above catalyst in a continuous trickle fixed bed reaction device;

[0075] (II) Maleic anhydride is placed in a solvent and mixed to obtain a reaction solution, and the reaction solution is injected into a continuous trickle fixed bed reactor under a reducing gas atmosphere to carry out a hydrogenation reduction reaction to obtain succinic anhydride.

[0076] The hydrogenation synthesis process of succinic anhydride provided by the present invention comprises the following steps: firstly placing the above-mentioned catalyst in a continuous trickle fixed bed reaction device, and then injecting the maleic anhydride reaction solution into the continuous trickle fixed bed reaction device under a reducing gas atmosphere for hydrogenation reduction reaction to obtain succinic anhydride. The hydrogenation synthesis method of the present application adopts a continuous trickle fixed bed hydrogenation process, which has the advantages of low reaction temperature and low hydrogen pressure, and can realize continuous production of succinic anhydride under mild conditions.

[0077] The technical solution of the present invention will be further described below in conjunction with embodiments.

[0078] Example 1: The forming carrier is alumina pellets

[0079] A catalyst, wherein the preparation method of the catalyst comprises:

[0080] (1) Weigh 1.70 g of nickel acetate tetrahydrate and dissolve it in 50 mL of ultrapure water to obtain a nickel acetate solution; at the same time, weigh 1.6 g of alumina ball carrier and add it to the above nickel nitrate solution, and stir for 4 hours to allow it to fully absorb the nickel nitrate salt;

[0081] (2) Add concentrated ammonia water while stirring to adjust the pH to 11-12, and continue stirring for 4 hours to allow the nickel nitrate in the solution to fully precipitate onto the alumina balls;

[0082] (3) Take out the nickel / alumina pellet precursor and dry it at 120° C. for 12 h;

[0083] (4) The nickel / alumina pellet precursor obtained above was placed in an alumina crucible and placed in a tube furnace. A 5% hydrogen-argon mixed gas was introduced at 25°C for 60 minutes to remove oxygen in the pipe, and then the temperature was raised to 450°C at a rate of 3°C / min, and reduced at 450°C for 3 hours in a 5% hydrogen-argon mixed atmosphere to prepare a nickel catalyst supported on alumina pellets (Ni / Al2O3-XQ).

[0084] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 1 was evaluated: 2 g of the Ni-Al2O3-1 mm catalyst in Example 1 was placed in a quartz tube and fixed to a continuous high-pressure reaction device. The hydrogen pressure in the reaction device system was adjusted to 0.5 MPa H2, maleic anhydride solution was pumped in at 120°C, and the mass space velocity was controlled to be 1.0 h -1 , run for 2 hours, collect the reaction solution and analyze it by gas chromatography. The results of gas chromatography analysis showed that the maleic anhydride conversion rate was 100% and the succinic anhydride yield was 99.1%.

[0085] Example 2: Investigation of molded carrier (silica spheres)

[0086] The preparation steps and material selection of this Example 2 are the same as those of Example 1, except that this Example 2 uses silica spheres (average particle size 1 mm) as the molding carrier, and the remaining preparation steps and material selection are the same as those of Example 1, to prepare a nickel catalyst (Ni / SiO2-XQ) loaded with silica spheres.

[0087] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 2 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 98.6%.

[0088] Example 3: Investigation of molded carrier (titanium dioxide spheres)

[0089] The preparation steps and material selection of this Example 3 are the same as those of Example 1, except that this Example 3 uses titanium dioxide spheres (average particle size 1 mm) as the forming carrier, and the remaining preparation steps and material selection are the same as those of Example 1, to prepare a nickel catalyst (Ni / TiO2-XQ) loaded with carbon dioxide spheres.

[0090] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 3 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 93.4%.

[0091] Example 4: Investigation of molded carrier (extruded activated carbon)

[0092] The preparation steps and material selection of this embodiment 4 are the same as those of embodiment 1, except that this embodiment 4 uses extruded activated carbon as a molding carrier, and the remaining preparation steps and material selection are the same as those of embodiment 1, to prepare an extruded activated carbon-supported nickel catalyst (Ni / C-JY).

[0093] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 4 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 99.4%.

[0094] Example 5: Investigation of molded carrier (hard carbon chips)

[0095] The preparation steps and material selection of this Example 5 are the same as those of Example 1, except that this Example 5 uses hard carbon crumbs as a forming carrier, and the remaining preparation steps and material selection are the same as those of Example 1, to prepare a hard carbon crumb-loaded nickel catalyst (Ni / C-TR).

[0096] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 5 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 99.9%.

[0097] The reaction data of Examples 1 to 5 for the continuous hydrogenation of maleic anhydride to succinic anhydride are summarized as shown in Table 1.

[0098] Table 1:

[0099]

[0100] It can be seen from the above table that the Ni / support shaped catalysts prepared by adsorption precipitation deposition using different shaped supports all have good effects on the continuous hydrogenation of maleic anhydride to succinic anhydride; among them, the catalyst prepared by titanium dioxide beads has a poor effect, and the yield of succinic anhydride is only 93.4%; this is because TiO2 will form a strong metal-support interaction (SMSI) during the calcination process, further wrapping the surface nickel nanoparticles, resulting in a decrease in the yield of succinic anhydride.

[0101] In summary, the adsorption-precipitation deposition method provided by the present invention is applicable to various types of shaped carriers and can be used to synthesize various types of high-performance shaped catalysts for continuous hydrogenation of maleic anhydride to succinic anhydride.

[0102] Among them: the Ni / C-TR catalyst prepared by the hard carbon crumb forming carrier in Example 5 has the best performance, and the yield of succinic anhydride reaches 99.9%.

[0103] Figure 1 This is a scanning electron microscope characterization image of the Ni / C-TR catalyst obtained in this example;

[0104] Figure 2 is the XRD characterization diagram of the Ni / C-TR catalyst obtained in this example;

[0105] Figure 3 This is the XPS characterization diagram of the Ni / C-TR catalyst obtained in this example;

[0106] Figure 4 This is a graph showing the stability test of maleic anhydride hydrogenation of the Ni / C-TR catalyst obtained in this example.

[0107] See also Figure 1 to Figure 4 Scanning electron microscopy showed that a large number of nickel-based nanoparticles ( Figure 1 ), and XRD characterization detected a clear diffraction peak signal of metallic nickel, indicating that the nickel nanoparticles prepared by the adsorption-precipitation deposition method provided by the present invention have a good crystal form ( Figure 2 ); Furthermore, XPS characterization detected obvious Ni 2P3 / 2 orbital binding energy signals ( Figure 3 ), further illustrating that the adsorption-precipitation deposition method provided by the present invention can effectively deposit nickel-based nanoparticles onto a shaped carrier.

[0108] By the above Figure 1 to Figure 3 The reaction mechanism of the catalyst of the present application is as follows: first, the nickel precursor is deposited on the surface of the carrier by the adsorption-precipitation deposition method, and is then reduced at high temperature to generate nickel nanocrystals with intact crystal structure that are adsorbed and formed on the surface of the carrier; during the hydrogenation process, hydrogen is adsorbed on the surface of these nickel nanocrystals and dissociated to form hydrogen atoms, and then maleic anhydride is adsorbed on the surface of the nickel nanocrystals and reacts with hydrogen atoms to hydrogenate to produce the target product, succinic anhydride.

[0109] See also Figure 4 The Ni / C-TR catalyst obtained in Example 5 was tested for stability under the same conditions. The catalyst could run stably for 200 h, and the yield of succinic anhydride was always maintained at above 99.8%, and no activity loss was observed ( Figure 4 ), which is due to the strong interaction between nickel nanoparticles and the carrier, which enables them to exist stably on the surface, thus ensuring the high hydrogenation stability of the catalyst.

[0110] In summary, the adsorption-precipitation deposition method provided by the present invention can effectively achieve uniform loading of metal nickel nanoparticles on the shaped carrier, thereby ensuring high activity and high stability of the catalyst.

[0111] Example 6: Investigation of alkaline precipitants (sodium carbonate)

[0112] The preparation steps and material selection of this embodiment 6 are the same as those of embodiment 1, except that this embodiment 6 uses sodium carbonate as a precipitant. The remaining preparation steps and material selection are the same as those of embodiment 1, and a nickel catalyst (Ni / Al2O3-XQ-Na2CO3) loaded with alumina beads is prepared.

[0113] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 6 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 99.2%.

[0114] Example 7: Investigation of alkaline precipitants (potassium carbonate)

[0115] The preparation steps and material selection of this embodiment 7 are the same as those of embodiment 1, except that potassium carbonate is used as a precipitant in this embodiment 7. The remaining preparation steps and material selection are the same as those of embodiment 1, and a nickel catalyst (Ni / Al2O3-XQ-K2CO3) loaded with alumina beads is prepared.

[0116] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 7 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 99.2%.

[0117] Example 8: Alkaline Precipitant Investigation (Sodium Hydroxide)

[0118] The preparation steps and material selection of this Example 8 are the same as those of Example 1, except that this Example 8 uses sodium hydroxide as a precipitant. The remaining preparation steps and material selection are the same as those of Example 1, and a nickel catalyst (Ni / Al2O3-XQ-NaOH) loaded with alumina beads is prepared.

[0119] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 8 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 98.6%.

[0120] Example 9: Investigation of alkaline precipitants (potassium hydroxide)

[0121] The preparation steps and material selection of this Example 9 are the same as those of Example 1, except that this Example 9 uses potassium hydroxide as a precipitant. The remaining preparation steps and material selection are the same as those of Example 1, and a nickel catalyst (Ni / Al2O3-XQ-KOH) supported on alumina beads is prepared.

[0122] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 9 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 98.7%.

[0123] Example 10: Investigation of alkaline precipitants (without using precipitants)

[0124] The preparation steps and material selection of this embodiment 10 are the same as those of embodiment 1, except that this embodiment 10 does not use a precipitant. The remaining preparation steps and material selection are the same as those of embodiment 1, and a nickel catalyst (Ni / Al2O3-XQ-WU) loaded with alumina beads is prepared.

[0125] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 10 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 90.4%.

[0126] Example 11: Investigation of alkaline precipitants (without using precipitants)

[0127] The preparation steps and material selection of this Example 11 are the same as those of Example 5, except that this Example 11 does not use a precipitant. The remaining preparation steps and material selection are the same as those of Example 5, and a nickel catalyst (Ni / C-TR-WU) supported on hard carbon crumbs is prepared.

[0128] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 11 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 98.9%.

[0129] The data of the continuous hydrogenation of maleic anhydride to succinic anhydride in Examples 6 to 11 are summarized in Table 2.

[0130] Table 2:

[0131]

[0132]

[0133] As can be seen from Table 2, for alumina pellets, the Ni / Al2O3-XQ shaped catalysts prepared using different alkaline precipitants all have excellent maleic anhydride continuous flow hydrogenation activity, and the succinic anhydride yields are all above 98%; when the precipitant is not used, the prepared Ni / Al2O3-XQ-WU shaped catalyst exhibits poor maleic anhydride continuous flow hydrogenation activity. The surface adsorption-precipitation deposition method can effectively allow the shaped carrier to adsorb more metal salt precursors, so the introduction of the precipitant further enhances the activity of the shaped catalyst; it is worth mentioning that for hard carbon debris, even without the addition of a precipitant, the Ni / C-TR-WU shaped catalyst still has excellent hydrogenation activity, and the succinic anhydride yield is close to 99%. This is because the activated carbon carrier has a strong adsorption capacity, and even without the introduction of a precipitant, it can completely adsorb the metal nickel salt in the solution, so the activity is not affected.

[0134] Example 12: Investigation of Metal Nickel Salt (Nickel Chloride Hexahydrate)

[0135] The preparation steps and material selection of this Example 12 are the same as those of Example 1, except that this Example 12 uses 1.6 g of nickel chloride hexahydrate as a precursor, and the remaining preparation steps and material selection are the same as those of Example 1, to prepare a nickel catalyst (Ni / Al2O3-XQ-Cl) loaded on alumina pellets.

[0136] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 12 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 99.1%.

[0137] Example 13: Investigation of Metal Nickel Salt (Nickel Nitrate Hexahydrate)

[0138] The preparation steps and material selection of this Example 13 are the same as those of Example 1, except that this Example 13 uses 1.98 g of nickel nitrate hexahydrate as a precursor, and the remaining preparation steps and material selection are the same as those of Example 1, to prepare a nickel catalyst loaded with alumina pellets (Ni / Al2O3-XQ-NO3).

[0139] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 12 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 99.0%.

[0140] Example 14: Investigation of Metal Nickel Salt (Nickel Acetylacetonate)

[0141] The preparation steps and material selection of this Example 14 are the same as those of Example 1, except that this Example 12 uses 1.75 g of nickel acetylacetonate as a nickel salt precursor dissolved in dilute ammonia water, and the remaining preparation steps and material selection are the same as those of Example 1, to prepare a nickel catalyst (Ni / Al2O3-XQ-AC) loaded with alumina pellets.

[0142] Hydrogenation catalytic efficiency: The performance of the catalyst prepared in Example 14 was evaluated. The catalytic reaction conditions were the same as those in Example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 100% and the succinic anhydride selectivity was 98.1%.

[0143] The reaction data of Examples 12 to 14 for continuous hydrogenation of maleic anhydride to succinic anhydride are summarized as shown in Table 3.

[0144] Table 3:

[0145]

[0146] As can be seen from Table 3, the Ni / Al2O3-XQ shaped catalysts prepared from different nickel salt precursors all have excellent maleic anhydride continuous flow hydrogenation activity, and the yield of succinic anhydride is more than 98%; it shows that the adsorption-precipitation deposition method provided by the present invention can not only be applied to different shaped carriers, but also to various metal salt precursors, and has wide universality; the catalyst synthesis process is simple, low cost, good performance, and has excellent activity and selectivity for the continuous hydrogenation of maleic anhydride to succinic anhydride; at the same time, the present invention adopts a continuous trickle fixed bed hydrogenation process, which is safe and reliable, with low reaction temperature and hydrogen pressure, mild conditions, and can achieve efficient and continuous production of succinic anhydride. In summary, the catalyst provided by the present invention, its preparation process, and the continuous trickle fixed bed hydrogenation process have broad industrial application prospects and are expected to be industrialized.

[0147] Comparative Example 1

[0148] In this comparative example 1, the alumina beads (average particle size 1 mm) used in this example 1 were used as catalysts. The catalytic reaction conditions were the same as those in example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 0%.

[0149] Comparative Example 2

[0150] In this comparative example 2, the silica beads (average particle size 1 mm) used in this example 2 were used as catalysts. The catalytic reaction conditions were the same as those in example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate was 0%.

[0151] Comparative Example 3

[0152] This comparative example 3 uses the titanium dioxide beads (average particle size 1 mm) used in this example 3 as a catalyst, and the catalytic reaction conditions are the same as those in example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate is 0%.

[0153] Comparative Example 4

[0154] This comparative example 4 uses the extruded activated carbon carrier used in this example 4 as the catalyst, and the catalytic reaction conditions are the same as those in example 1. According to the results of gas chromatography analysis, the maleic anhydride conversion rate is 0%.

[0155] Comparative Example 5

[0156] In this comparative example 5, the hard carbon crumbs used in this example 5 were used as catalysts. The catalytic reaction conditions were the same as those in example 1. According to the results of gas chromatography analysis, the conversion rate of maleic anhydride was 0%.

[0157] Comparative Examples 1 to 5 are used for the continuous hydrogenation of maleic anhydride to succinic anhydride reaction data summary: see Table 4.

[0158] Table 4:

[0159]

[0160] It can be seen from Table 4 that different shaped carriers that have not adsorbed nickel nanoparticles by the adsorption-precipitation deposition method have no maleic anhydride hydrogenation activity, indicating that without the deposition of nickel-based nanoparticles, the carrier has no hydrogenation activity. The adsorption-precipitation deposition method provided by the present invention is an effective method for preparing a high-activity and high-stability shaped nickel-based catalyst for hydrogenation of maleic anhydride to succinic anhydride.

[0161] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A catalyst, characterized in that The catalyst comprises a carrier and a metal nickel-based active component, wherein the metal nickel-based active component is nickel nanoparticles loaded on the carrier.

2. The catalyst according to claim 1, characterized in that The carrier includes any one of alumina beads, silica beads, titania beads or shaped carbon crumbs, or a combination of at least two of them.

3. The catalyst according to claim 2, characterized in that The molded carbon crumbs are obtained by mixing activated carbon powder with a strengthening agent, a binder, and a pore-forming agent, and then extruding and molding; Preferably, the strengthening agent comprises any one or a combination of at least two of glass fiber, aluminum oxide or silicon oxide; Preferably, the binder comprises any one or a combination of at least two of hydroxypropyl cellulose, hydroxymethyl cellulose, polyvinyl alcohol, gum, sesbania powder, aluminum sol or silica sol; Preferably, the pore-forming agent comprises any one of dry starch, polyethylene glycol, polyethylene oxide, paraffin or glycerol, or a combination of at least two thereof.

4. The catalyst according to claim 1, characterized in that The 2p 3 / 2 orbital binding energy of the nickel element in the nickel nanoparticles is 849 eV to 868 eV.

5. A method for preparing a catalyst according to any one of claims 1 to 4, characterized in that: The preparation method comprises: (A) adding a carrier to a metal nickel salt solution and mixing, then adding an alkaline precipitant to precipitate the metal nickel salt onto the carrier, and drying to obtain a precursor A; (B) Under reducing atmosphere conditions, the precursor A is calcined and reduced to obtain the catalyst.

6. The method for preparing the catalyst according to claim 5, characterized in that: The metal nickel salt in the metal nickel salt solution of step (A) comprises any one of nickel chloride, nickel nitrate, nickel acetate, nickel formate or nickel acetylacetonate, or a combination of at least two thereof; Preferably, the solvent in the metal nickel salt solution in step (A) comprises any one of water, methanol, ethanol, tetrahydrofuran or N,N-dimethylformamide, or a combination of at least two thereof; Preferably, the alkaline precipitant in step (A) comprises any one of ammonia solution, alkali metal hydroxide or alkali metal carbonate, or a combination of at least two thereof; Preferably, the ammonia solution is aqueous ammonia and / or a methanol solution of ammonia; Preferably, the alkali metal hydroxide comprises sodium hydroxide and / or potassium hydroxide; Preferably, the alkali metal carbonate comprises sodium carbonate and / or potassium carbonate.

7. The method for preparing a catalyst according to claim 5, characterized in that: The reducing atmosphere in step (B) comprises any one of hydrogen, hydrogen / argon mixed gas, carbon monoxide, methane or acetylene, or a combination of at least two thereof; Preferably, the temperature of the calcination reduction in step (B) is 100-600°C; Preferably, the calcination reduction time in step (B) is 1 to 12 hours.

8. Use of the catalyst according to any one of claims 1 to 4, or the catalyst prepared according to the preparation method according to any one of claims 5 to 7 as a catalyst for preparing succinic anhydride by hydrogenation reduction.

9. A method for preparing succinic anhydride, characterized in that: The preparation method comprises: In the presence of the catalyst according to any one of claims 1 to 4 or the catalyst prepared by the preparation method according to any one of claims 5 to 7, maleic anhydride is subjected to a hydrogenation reduction reaction to obtain succinic anhydride.

10. The method for preparing succinic anhydride according to claim 9, characterized in that: The preparation method specifically comprises the following steps: (I) placing the catalyst according to any one of claims 1 to 4 or the catalyst prepared by the preparation method according to any one of claims 5 to 7 in a continuous trickle fixed bed reaction device; (II) Maleic anhydride is placed in a solvent and mixed to obtain a reaction solution, and the reaction solution is injected into a continuous trickle fixed bed reactor under a reducing gas atmosphere to carry out a hydrogenation reduction reaction to obtain succinic anhydride.

Citation Information

Patent Citations

  • Catalyst for continuous production of succinic anhydride from hydrogenation of maleic anhydride and preparation method thereof

    CN101502802A

  • Continuous production process for preparing succinyl oxide by maleic anhydride hydrogenation

    CN101891718A

  • Catalyst for catalyzing maleic anhydride and hydrogenating to prepare butanedioic anhydride under low temperature and low pressure and preparation method of catalyst

    CN104399469A

  • Catalyst for catalyzing hydrogenation of petroleum resin as well as preparation method and application thereof

    CN105413694A

  • Composite high-efficiency catalyst for preparing succinic anhydride through maleic anhydride body hydrogenation and preparation method of composite high-efficiency catalyst

    CN113231069A