Red mud-based VOCs (volatile organic compounds) pretreating agent as well as preparation method and application thereof
The red mud-based VOCs pretreatment agent addresses the challenge of simultaneous sulfur and silicone treatment by forming a Fe-Sn-Al system, capturing Si and S, and adsorbing SO2, thus enhancing catalyst resistance and resource utilization.
Patent Information
- Application Number
- CN202411421817.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-12
AI Technical Summary
Existing VOCs pretreatment agents are ineffective in simultaneously treating sulfur and silicone-containing waste gases, leading to rapid catalyst deactivation and high production costs, while red mud, a waste residue, lacks effective utilization.
A red mud-based VOCs pretreatment agent is developed by adding Sn to form a Fe-Sn-Al system, enhancing sulfur resistance and capturing silicon and sulfur components, with red mud's alkaline components adsorbing SO2 to form sulfates, reducing poisoning effects on downstream catalysts.
The pretreatment agent effectively captures Si and S, alleviating catalyst poisoning, promoting resource utilization of red mud, and reducing pollution, while maintaining catalyst efficiency and lowering production costs.
Smart Images

Figure CN119076003A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of VOCs catalysts, and specifically relates to a red mud-based VOCs pretreatment agent and a preparation method and application thereof. Background Art
[0002] Volatile organic compounds (VOCs) are one of the main causes of haze, atmospheric photochemical smog, greenhouse effect and ozone layer depletion. Their emission sources are mainly human-induced, mostly caused by the production process, fuel combustion process and product consumption behavior of petrochemical related industries. Among them, VOCs waste gas from industries such as silicone rubber contains sulfur and organosilicon, which leads to silicon poisoning and sulfur poisoning of catalysts in catalytic oxidation treatment processes, causing the catalyst to be quickly poisoned and deactivated.
[0003] The preparation of VOCs pretreatment agents in the prior art is mainly aimed at single silicon-containing organic waste gas, and rarely involves VOCs pretreatment agents that can simultaneously treat sulfur and silicone; at the same time, the existing VOCs pretreatment agent preparation method is mostly prepared by vacuum coating. The pretreatment capacity of the pretreatment agent prepared by this method is limited by the coating load, and it is difficult to meet the treatment needs of the continuously accumulated VOCs. Although there are a few coping methods, for example: Patent CN 114100669A discloses an extruded 400-mesh honeycomb silicon-containing VOCs pretreatment catalyst, including an aluminum-based carrier, an active component and other additives. Although the catalyst can protect the rear-end precious metal catalyst, its extrusion production process and high mesh count characteristics greatly increase the production cost, and it is not suitable for working conditions containing sulfur and silicone at the same time.
[0004] Red mud is a harmful waste residue produced in the industrial aluminum production process. Its main chemical components include: Fe2O 3、 Al2O3, TiO2, SiO2, Na2O, MgO, and many other elements such as Cu, Mn, V, Zr, K. Due to the large amount of red mud produced and limited application methods, a large amount of red mud cannot be effectively utilized and can only be piled up in the yard, occupying a large amount of land resources and causing pollution to the atmosphere, water resources and soil. Therefore, how to realize the resource utilization of red mud has become a difficult problem to be solved in the aluminum smelting industry. Iron-based catalysts have good redox properties and water resistance. Some studies have prepared denitrification catalysts with red mud rich in Fe2O3, but the red mud needs to be subjected to complex dealkalization treatment to reduce the influence of alkaline components (such as Na2O, K2O, etc.) on the denitrification performance. Summary of the invention
[0005] The purpose of the present invention is to provide a red mud-based VOCs pretreatment agent, thereby overcoming the shortcomings of the prior art. By directly adding Sn to red mud to construct a Fe-Sn-Al sulfur-containing organosilicon pretreatment system, the anti-sulfur performance of Fe2O3 and Al2O3 is improved, and the silicon element in VOCs is captured on the aluminum site of the pretreatment agent to form silicon dioxide crystals; the alkaline components in red mud can effectively adsorb sulfur dioxide (SO2) in VOCs to form sulfates, effectively reducing the poisoning effect of organosilicon and SO2 in VOCs in the silicone rubber industry on the back-end precious metal or non-precious metal catalysts.
[0006] In order to achieve the above object, the technical solution of the present invention is: In a first aspect, the present invention provides a red mud-based VOCs pretreatment agent, wherein the components of the red mud-based VOCs pretreatment agent are, by weight, 70-90 parts of red mud, 5-20 parts of Sn precursor, 5-10 parts of auxiliary agent, and 20-40 parts of water.
[0007] In some other embodiments, the Sn precursor is one or more of tin chloride, stannous chloride or sodium stannate; Alternatively, the particle size D90 of the red mud is 5-50 μm.
[0008] In some other embodiments, the auxiliary agent is one or more of glass fiber, silica sol, aluminum sol, hydroxypropyl methylcellulose, methyl cellulose, ethylene glycol, polyethylene glycol, polyvinyl alcohol, polyethylene oxide, polyacrylamide or mineral oil.
[0009] The inventors found in their research that the red mud obtained by the Bayer process has a large specific surface area, a porous skeleton structure, and contains 15-40 wt.% Al2O3, which has the potential to be used in the pretreatment of organic silicon in the field of VOCs catalytic combustion. The addition of tin precursors facilitates the construction of the Fe-Sn-Al system, and utilizes the interaction between Fe, Sn, and Al to increase the electrophobicity of the Fe-Al surface, inhibit the transfer of electrons on SO2 to the Fe-Al site, thereby reducing the adsorption of SO2 on the Fe-Al surface and the formation of sulfates. The addition of additives can enhance the mechanical strength, microporous structure and specific surface area of red mud-based VOCs pretreatment agents; at the same time, the organic matter in the additives is removed during the roasting process to form a pore structure. The rich pore structure is conducive to increasing the contact area and time between the pretreatment agent and the VOCs exhaust gas, thereby improving the pretreatment effect.
[0010] In a second aspect, the present invention provides a method for preparing the red mud-based VOCs pretreatment agent according to the first aspect, comprising the following steps: (1) mixing red mud, Sn precursor, additive and water to obtain a mixture; (2) kneading the mixture to obtain a clay material; (3) Extruding and cutting the clay material to obtain a pretreatment agent wet embryo; (4) The red mud-based VOCs pretreatment agent is obtained by drying and calcining the wet pretreatment agent.
[0011] In some other embodiments, in step (2), the mixing time is 0.5-2h; after the mixing is completed, a screening process is also performed, and the screening process is sequentially performed by roughing and screening, aging, and refining and screening; The filter mesh specification of the coarse refining and screening is 25-100 mesh, the aging time is 6-24h, and the filter mesh specification of the refined refining and screening is 100-200 mesh.
[0012] In some other embodiments, in step (3), the shape of the pretreatment agent wet embryo is a cuboid, a cube or a cylinder; The cross-sectional opening number of the wet embryo of the pretreatment agent is 100-400 meshes and the length is 50-300 mm, thereby ensuring that the pressure loss of the pretreatment agent is consistent with that of a conventional VOCs catalyst.
[0013] In some other embodiments, in step (4), the drying is microwave drying, the power of microwave drying is 50-500 W, and the time of microwave drying is 10-120 min; Alternatively, the calcination temperature is 400-600° C., and the calcination time is 2-15 hours.
[0014] In a third aspect, the present invention provides the use of the red mud-based VOCs pretreatment agent described in the first aspect in treating VOCs gas.
[0015] In some other embodiments, the red mud-based VOCs pretreatment agent is used to simultaneously capture Si and S in the VOCs gas, thereby reducing the contact of organic silicon and SO2 in the VOCs with the rear-end precious metal or non-precious metal catalyst.
[0016] In a fourth aspect, the present invention provides a method for treating VOCs, wherein the red mud-based VOCs pretreatment agent described in the first aspect is installed at the front end or upstream of the VOCs catalyst.
[0017] Beneficial effects of the present invention: (1) The present invention prepares a pretreatment agent for the pretreatment of sulfur-containing and organosilicon VOCs gases in the silicone rubber industry by doping Bayer red mud with Sn. The organosilicon VOCs are first captured by the Al site of Al2O3 and then oxidized to SiO2 by Fe2O3 and accumulated on the surface of the pretreatment agent, thereby significantly reducing the organosilicon content in the gas and effectively alleviating the silicon poisoning problem of the back-end precious metal catalyst. (2) The Bayer red mud used in the present invention does not require complex and costly dealkalization treatment. The alkaline components (such as Na2O, K2O, etc.) contained in the red mud can efficiently adsorb SO2 in the VOCs gas to generate sulfate, thereby significantly reducing the SO2 content in the gas and effectively alleviating the sulfur poisoning problem of the back-end precious metal catalyst. On the other hand, by adding Sn to construct the Fe-Sn-Al oxide system, the sulfur resistance of Fe2O3 and Al2O3 is improved, thereby maintaining the high-efficiency silicone pretreatment capability. (3) The present invention can realize the resource utilization of red mud and reduce the pollution of red mud to the natural environment. At the same time, the pretreatment agent prepared by the present invention can realize the pretreatment of sulfur-containing and silicone VOCs in the silicone rubber industry, avoiding the rapid deactivation of VOCs precious metal catalysts and causing economic losses, which is conducive to promoting the application of catalytic combustion technology to replace part of the direct combustion technology in the field of silicone rubber VOCs waste gas treatment, and realizing the reduction of pollution and carbon emissions in VOCs treatment.
[0018] (4) The preparation method of the present invention is simple, practical and easy to promote. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0020] Figure 1 The SEM-EDS mapping spectrum of the pretreatment agent prepared in Example 1 of the present invention before and after the reaction, wherein a is the surface Si element before the reaction, b is the surface Si element after the reaction, c is the surface S element before the reaction, and d is the surface S element after the reaction; Figure 2 The efficiency diagram of the combination of the pretreatment agent prepared in Examples 1 and 2 and Comparative Examples 1 and 3 of the present invention and the VOCs precious metal catalyst for catalyzing ethyl acetate and hexamethyldisiloxane; among them, Example 1 Sample I, Example 2 Sample II, Comparative Example 1 Sample VI, Comparative Example 3 Sample VIII. DETAILED DESCRIPTION
[0021] Example 1 A method for preparing a red mud-based VOCs pretreatment agent comprises the following steps: Step (1): weighing 85 parts of Bayer red mud, 10 parts of stannous chloride, 5 parts of additives (2 parts of glass fiber, 1 part of hydroxypropyl methylcellulose, 1 part of polyethylene glycol and 1 part of mineral oil) and 25 parts of water to obtain a mixture; Step (2): the mixture of step 1 is transferred to a mixer and mixed for 1 hour, and then sieved through a 60-mesh filter, aged for 8 hours, and refined through a 120-mesh filter to obtain a slurry; Step (3): Extruding the clay material of step 2 through an extruder, and cutting it to obtain a pretreatment agent wet embryo with a cross-sectional opening number of 300 meshes and a length of 50 mm; Step (4): subjecting the wet embryo from step 3 to microwave drying, with a microwave drying power of 200 W and a drying time of 40 min; and finally calcining at 550° C. for 4 h to prepare a red mud-based VOCs pretreatment agent I.
[0022] Figure 1 The SEM-mapping spectrum of the pretreatment agent prepared in Example 1 of the present invention before and after the reaction, wherein a is the surface Si element before the reaction, b is the surface Si element after the reaction, c is the surface S element before the reaction, and d is the surface S element after the reaction. Figure 1 It can be seen that after the reaction, Si and S elements are evenly and densely distributed on the surface of the pretreatment agent, which proves that the pretreatment agent prepared by the invention can achieve the pretreatment of sulfur-containing and silicone VOCs in the silicone rubber industry.
[0023] The axial compressive strength of the pretreatment agent was measured to be 4.1 MPa, the radial compressive strength was 1.1 MPa, and the specific surface area was 83 m 2 / g.
[0024] Example 2 The difference from Example 1 is that stannous chloride is not added; in step (1), 95 parts of Bayer red mud, 5 parts of additives (2 parts of glass fiber, 1 part of hydroxypropyl methylcellulose, 1 part of polyethylene glycol and 1 part of mineral oil) and 25 parts of water are weighed and mixed; The other preparation steps were consistent with those in Example 1 to prepare red mud-based VOCs pretreatment agent II.
[0025] The axial compressive strength of the pretreatment agent was measured to be 4.2MPa, the radial compressive strength was 1.1MPa, and the specific surface area was 82m 2 / g.
[0026] Example 3 The difference from Example 1 is that in step (3), the clay material in step (2) is extruded and cut into a pretreatment agent wet embryo with a cross-sectional opening number of 200 meshes and a length of 50 mm. The other preparation steps were consistent with those in Example 1 to prepare red mud-based VOCs pretreatment agent III.
[0027] The axial compressive strength of the pretreatment agent was measured to be 3.6 MPa, the radial compressive strength was 0.9 MPa, and the specific surface area was 82 m 2 / g.
[0028] Example 4 The difference from Example 1 is that in step (3), the mud material in step (2) is extruded and formed by an extruder, and cut to obtain a pretreatment agent wet embryo with a cross-sectional opening number of 300 meshes and a length of 200 mm; In step (4), the wet embryo in step (3) is subjected to microwave drying, the microwave drying power is 400 W, and the drying time is 100 min; and finally, it is roasted at 550° C. for 9 h; The other preparation steps were consistent with those in Example 1 to prepare red mud-based VOCs pretreatment agent IV.
[0029] The axial compressive strength of the pretreatment agent was measured to be 4.2MPa, the radial compressive strength was 1.2MPa, and the specific surface area was 85m 2 / g.
[0030] Example 5 The difference from Example 1 is that in step (1), 85 parts of Bayer process red mud, 10 parts of stannous chloride, 5 parts of additives (respectively 1 part of silica sol, 1 part of methyl cellulose, 1 part of polyvinyl alcohol, 1 part of polyethylene oxide and 1 part of polyacrylamide) and 25 parts of water are weighed and mixed; The other preparation steps were consistent with those in Example 1 to prepare red mud-based VOCs pretreatment agent V.
[0031] The axial compressive strength of the pretreatment agent was measured to be 3.5MPa, the radial compressive strength was 0.8MPa, and the specific surface area was 89m 2 / g.
[0032] Comparative Example 1 The difference from Example 1 is that in step (1), 50 parts of Fe2O3, 35 parts of Al2O3, 10 parts of stannous chloride, 5 parts of additives (2 parts of glass fiber, 1 part of hydroxypropyl methylcellulose, 1 part of polyethylene glycol, and 1 part of mineral oil) and 25 parts of water are weighed and mixed; The other preparation steps were consistent with those in Example 1 to prepare red mud-based VOCs pretreatment agent VI.
[0033] The axial compressive strength of the pretreatment agent was measured to be 3.8MPa, the radial compressive strength was 0.9MPa, and the specific surface area was 57m 2 / g.
[0034] Comparative Example 2 The difference from Example 1 is that in step (1), 56 parts of Fe2O3, 39 parts of Al2O3, 5 parts of additives (2 parts of glass fiber, 1 part of hydroxypropyl methylcellulose, 1 part of polyethylene glycol and 1 part of mineral oil) and 25 parts of water are weighed and mixed; The other preparation steps were the same as those in Example 1 to prepare red mud-based VOCs pretreatment agent VII.
[0035] The axial compressive strength of the pretreatment agent was measured to be 3.8MPa, the radial compressive strength was 0.8MPa, and the specific surface area was 56m 2 / g.
[0036] Comparative Example 3 The difference from Example 1 is that in step (1), 85 parts of Bayer red mud, 10 parts of ammonium heptamolybdate, 5 parts of additives (2 parts of glass fiber, 1 part of hydroxypropyl methylcellulose, 1 part of polyethylene glycol and 1 part of mineral oil) and 25 parts of water are weighed and mixed; The other preparation steps were consistent with those in Example 1 to prepare red mud-based VOCs pretreatment agent VIII.
[0037] The axial compressive strength of the pretreatment agent was measured to be 4.0 MPa, the radial compressive strength was 1.0 MPa, and the specific surface area was 78 m 2 / g.
[0038] Comparative Example 4 The difference from Example 1 is that no auxiliary agent is added; in step (1), 90 parts of Bayer process red mud, 5 parts of stannous chloride and 25 parts of water are weighed and mixed; The other preparation steps were consistent with those in Example 1 to prepare red mud-based VOCs pretreatment agent IX.
[0039] The axial compressive strength of the pretreatment agent was measured to be 1.4 MPa, the radial compressive strength was 0.2 MPa, and the pore size was 45 m 2 / g.
[0040] Comparative Example 5 The difference from Example 1 is that in step (1), 85 parts of Bayer red mud, 10 parts of stannous chloride, 5 parts of additives (3 parts of glass fiber and 2 parts of hydroxypropyl methylcellulose) and 25 parts of water are weighed and mixed; The other preparation steps are consistent with Example 1 to prepare red mud-based VOCs pretreatment agent X.
[0041] The axial compressive strength of the pretreatment agent was measured to be 4.7 MPa, the radial compressive strength was 1.2 MPa, and the pore size was 64 m 2 / g.
[0042] Comparative Example 6 The difference from Example 1 is that in step (1), 85 parts of Bayer process red mud, 10 parts of stannous chloride, 5 parts of additives (2 parts of polyethylene glycol and 3 parts of mineral oil) and 25 parts of water are weighed and mixed; The other preparation steps were the same as those in Example 1 to prepare the red mud-based VOCs pretreatment agent XI.
[0043] The axial compressive strength of the pretreatment agent was measured to be 0.9MPa, the radial compressive strength was 0.1MPa, and the specific surface area was 96m 2 / g.
[0044] Performance Verification: The red mud-based VOCs pretreatment agents prepared in the examples and comparative examples were tested. A cylindrical honeycomb sample (φ30*50mm) was cut using the pretreatment agents prepared in Examples 1-5 and Comparative Examples 1-3, and a rotary concentrated VOCs noble metal catalyst commercially available from Jiangsu Zhongchuang Qingyuan Technology Co., Ltd. The pretreatment agent was placed in front of the VOCs noble metal catalyst in series with it, and the activity of the VOCs catalyst changed over time after the addition of the pretreatment agent.
[0045] Test conditions: reaction temperature: 300°C, ethyl acetate concentration: 1000ppm, hexamethyldisiloxane concentration: 300ppm, SO2 concentration: 500ppm, volume space velocity: 15000 h -1 ; The time when the catalytic VOCs conversion rate drops to 90% is recorded as t90 (h), and the time when the conversion rate drops to 50% is recorded as t50 (h). Table 1 shows the conversion performance of the pretreatment agent and the change data of Si and S content before and after the reaction.
[0046] Table 1 Conversion performance of pretreatment agent and changes in Si and S content before and after reaction
[0047] Table 1 shows the conversion performance of the pretreatment agent and the change data of Si and S content before and after the reaction. It is not difficult to see from Table 1 that the catalyst after adding the pretreatment agent sample Ⅺ prepared in Comparative Example 6 has the longest activity time, but the sample strength is significantly reduced and cannot meet the requirements for the strength and specific surface area of the pretreatment agent in practical applications (the axial compressive strength is required to be ≥2MPa, the radial compressive strength is ≥0.2MPa, and the specific surface area is ≥50m 2 / g). The performance of the pretreatment agent prepared in Example 4 is close to that of Comparative Example 6 and has higher strength, so the pretreatment agent prepared in Example 4 has the best performance; while in Example 2, since no stannous chloride is added, the Fe-Sn-Al system cannot be constructed, resulting in the adsorption of SO2 on the Fe-Al surface and the formation of sulfate, which leads to a significant reduction in the activity time of the catalyst, which is consistent with the results of the change in Si and S content of the pretreatment agent before and after the reaction. The number of openings in the wet embryo section of the pretreatment agent prepared in Example 3 is 200 mesh, which is lower than the number of openings in the wet embryo section of the pretreatment agent in Example 1 (300 mesh), resulting in a reduction in the surface area of the pretreatment agent. During the test, the surface flow rate of the sample increases, thereby reducing the ability to adsorb SO2 and silicone in VOCs gas, resulting in a reduction in the activity time of the catalyst.
[0048] The pretreatment agent prepared in Comparative Examples 1-3 has a poor effect on the use activity of the catalyst. This is because the conventional Fe2O3 and Al2O3 as raw materials do not contain the alkaline components contained in the red mud (such as Na2O, K2O, etc.) compared with the Bayer red mud, so it is not possible to efficiently adsorb SO2 in the VOCs gas, and the formation of sulfate leads to reduced catalyst activity; in addition, the addition of other types of transition metal salts such as ammonium heptamolybdate cannot construct the Fe-Sn-Al oxide system, improve the anti-sulfur performance of Fe2O3 and Al2O3, and thus maintain the efficient organosilicon pretreatment ability. It can be seen from Comparative Examples 4-6 that the addition of additives can enhance the mechanical strength, microporous structure and specific surface area of the red mud-based VOCs pretreatment agent; at the same time, the organic matter in the additive is removed during the roasting process to form a pore structure, and the rich pore structure is conducive to increasing the contact area and time between the pretreatment agent and the VOCs waste gas, thereby improving the pretreatment effect.
[0049] Figure 2 The efficiency diagram of the combination of the pretreatment agent prepared in Examples 1 and 2 of the present invention and Comparative Examples 1 and 3 and the VOCs noble metal catalyst for catalyzing ethyl acetate and hexamethyldisiloxane.
[0050] From Table 1 and Figure 2 It can be seen that the red mud-based organosilicon VOCs pretreatment agent prepared by Sn doping Bayer red mud accumulates the highest content of sulfur and silicon elements, so that the pretreatment agent + VOCs noble metal catalyst combination shows the best anti-sulfur poisoning and anti-organosilicon poisoning performance. Under this atmosphere condition, the VOCs noble metal catalyst activity is higher than 90% for about 6.7 hours, and the catalyst runs for about 8.0 hours when the catalytic activity decays to 50%. The pretreatment effect of the implementation sample II prepared without Sn doping is significantly lower than that of the implementation samples I, III, IV and V. Comparative sample VI and VII prepared by replacing Bayer red mud with Fe2O3 and Al2O3, and comparative sample VIII prepared by replacing Sn with Mo, cannot effectively extend the service life of the VOCs noble metal catalyst under the condition of the simultaneous presence of SO2 and organosilicon.
[0051] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A red mud-based VOCs pretreatment agent, It is characterized in that Calculated by weight, the components of the red mud-based VOCs pretreatment agent are: 70-90 parts of red mud, 5-20 parts of Sn precursor, 5-10 parts of auxiliary agent, and 20-40 parts of water.
2. The red mud-based VOCs pretreatment agent according to claim 1, It is characterized in that The Sn precursor is one or more of tin chloride, stannous chloride or sodium stannate; Alternatively, the particle size D90 of the red mud is 5-50 μm.
3. The red mud-based VOCs pretreatment agent according to claim 1, It is characterized in that The auxiliary agent is one or more of glass fiber, silica sol, aluminum sol, hydroxypropyl methylcellulose, methyl cellulose, ethylene glycol, polyethylene glycol, polyvinyl alcohol, polyethylene oxide, polyacrylamide or mineral oil.
4. A method for preparing the red mud-based VOCs pretreatment agent according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) mixing red mud, Sn precursor, additive and water to prepare a mixture; (2) kneading the mixture to obtain a clay material; (3) Extruding and cutting the clay material to obtain a pretreatment agent wet embryo; (4) The red mud-based VOCs pretreatment agent is obtained by drying and calcining the wet pretreatment agent.
5. The method for preparing the red mud-based VOCs pretreatment agent according to claim 4, It is characterized in that In step (2), the mixing time is 0.5-2h; after the mixing is completed, a screening process is also performed, and the screening process is to sequentially perform roughing screening, aging, and refining screening to obtain a mud material; The filter mesh specification of the coarse refining and screening is 25-100 mesh, the aging time is 6-24h, and the filter mesh specification of the refined refining and screening is 100-200 mesh.
6. The method for preparing the red mud-based VOCs pretreatment agent according to claim 4, It is characterized in that In step (3), the shape of the pretreatment agent wet embryo is a cuboid, a cube or a cylinder; The cross-sectional opening number of the wet embryo of the pretreatment agent is 100-400 meshes and the length is 50-300 mm.
7. The method for preparing the red mud-based VOCs pretreatment agent according to claim 4, It is characterized in that In step (4), the drying is microwave drying, the power of microwave drying is 50-500 W, and the microwave drying time is 10-120 min; Alternatively, the calcination temperature is 400-600° C., and the calcination time is 2-15 hours.
8. Use of the red mud-based VOCs pretreatment agent according to any one of claims 1 to 3 in treating VOCs gas.
9. The use as claimed in claim 8, It is characterized in that The red mud-based VOCs pretreatment agent is used to simultaneously capture Si and S in VOCs gas, reduce organic silicon and SO in VOCs 2 Contact with back-end precious metal or non-precious metal catalysts.
10. A method for treating VOCs. It is characterized in that The red mud-based VOCs pretreatment agent according to any one of claims 1 to 3 is installed at the front end or upstream of the VOCs catalyst.
Citation Information
Patent Citations
Catalyst prepared from red mud for removing volatile organic compound and preparation method of catalyst
CN108043404A
Fly-ash-based catalyst for catalytic combustion of VOCs and preparation method of catalyst
CN108816236A
Sulfur-tolerant volatile organic compound combustion catalyst and preparation method and application thereof
CN112871164A
Method for preparing honeycomb molecular sieve adsorbent from red mud
CN113368813A
Silicon-containing VOCs (volatile organic compounds) pretreatment agent as well as preparation method and application thereof
CN118616110A